WO2021049576A1 - 光造形用樹脂組成物、モデル材組成物、およびその光硬化物、ならびに光造形用組成物セット - Google Patents
光造形用樹脂組成物、モデル材組成物、およびその光硬化物、ならびに光造形用組成物セット Download PDFInfo
- Publication number
- WO2021049576A1 WO2021049576A1 PCT/JP2020/034322 JP2020034322W WO2021049576A1 WO 2021049576 A1 WO2021049576 A1 WO 2021049576A1 JP 2020034322 W JP2020034322 W JP 2020034322W WO 2021049576 A1 WO2021049576 A1 WO 2021049576A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- mass
- parts
- stereolithography
- monomer
- resin composition
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Ceased
Links
Classifications
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
- B29C64/00—Additive manufacturing, i.e. manufacturing of three-dimensional [3D] objects by additive deposition, additive agglomeration or additive layering, e.g. by 3D printing, stereolithography or selective laser sintering
- B29C64/10—Processes of additive manufacturing
- B29C64/106—Processes of additive manufacturing using only liquids or viscous materials, e.g. depositing a continuous bead of viscous material
- B29C64/112—Processes of additive manufacturing using only liquids or viscous materials, e.g. depositing a continuous bead of viscous material using individual droplets, e.g. from jetting heads
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B33—ADDITIVE MANUFACTURING TECHNOLOGY
- B33Y—ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- B33Y70/00—Materials specially adapted for additive manufacturing
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
- B29C64/00—Additive manufacturing, i.e. manufacturing of three-dimensional [3D] objects by additive deposition, additive agglomeration or additive layering, e.g. by 3D printing, stereolithography or selective laser sintering
- B29C64/40—Structures for supporting 3D objects during manufacture and intended to be sacrificed after completion thereof
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B33—ADDITIVE MANUFACTURING TECHNOLOGY
- B33Y—ADDITIVE MANUFACTURING, i.e. MANUFACTURING OF THREE-DIMENSIONAL [3D] OBJECTS BY ADDITIVE DEPOSITION, ADDITIVE AGGLOMERATION OR ADDITIVE LAYERING, e.g. BY 3D PRINTING, STEREOLITHOGRAPHY OR SELECTIVE LASER SINTERING
- B33Y80/00—Products made by additive manufacturing
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08F—MACROMOLECULAR COMPOUNDS OBTAINED BY REACTIONS ONLY INVOLVING CARBON-TO-CARBON UNSATURATED BONDS
- C08F220/00—Copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical or a salt, anhydride ester, amide, imide or nitrile thereof
- C08F220/02—Monocarboxylic acids having less than ten carbon atoms; Derivatives thereof
- C08F220/10—Esters
- C08F220/12—Esters of monohydric alcohols or phenols
- C08F220/16—Esters of monohydric alcohols or phenols of phenols or of alcohols containing two or more carbon atoms
- C08F220/18—Esters of monohydric alcohols or phenols of phenols or of alcohols containing two or more carbon atoms with acrylic or methacrylic acids
- C08F220/1811—C10or C11-(Meth)acrylate, e.g. isodecyl (meth)acrylate, isobornyl (meth)acrylate or 2-naphthyl (meth)acrylate
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L33/00—Compositions of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides or nitriles thereof; Compositions of derivatives of such polymers
- C08L33/04—Homopolymers or copolymers of esters
- C08L33/06—Homopolymers or copolymers of esters of esters containing only carbon, hydrogen and oxygen, which oxygen atoms are present only as part of the carboxyl radical
-
- C—CHEMISTRY; METALLURGY
- C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
- C08L—COMPOSITIONS OF MACROMOLECULAR COMPOUNDS
- C08L79/00—Compositions of macromolecular compounds obtained by reactions forming in the main chain of the macromolecule a linkage containing nitrogen with or without oxygen or carbon only, not provided for in groups C08L61/00 - C08L77/00
- C08L79/04—Polycondensates having nitrogen-containing heterocyclic rings in the main chain; Polyhydrazides; Polyamide acids or similar polyimide precursors
-
- B—PERFORMING OPERATIONS; TRANSPORTING
- B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
- B29K—INDEXING SCHEME ASSOCIATED WITH SUBCLASSES B29B, B29C OR B29D, RELATING TO MOULDING MATERIALS OR TO MATERIALS FOR MOULDS, REINFORCEMENTS, FILLERS OR PREFORMED PARTS, e.g. INSERTS
- B29K2105/00—Condition, form or state of moulded material or of the material to be shaped
- B29K2105/24—Condition, form or state of moulded material or of the material to be shaped crosslinked or vulcanised
Definitions
- the present invention relates to a resin composition for stereolithography used in a stereolithography method and a photocured product of the resin composition for stereolithography.
- the present invention also relates to a model material composition used in the material jet stereolithography method, a photocured product of the model material composition, and a composition set for material jet stereolithography including the model material composition.
- a method of producing a three-dimensional model by irradiating a photocurable resin composition with light such as ultraviolet rays to continuously form a cured layer having a predetermined shape is widely known.
- the stereolithography method include a stereolithography method using a liquid tank photopolymerization method in which a liquid photocurable resin is irradiated with light such as ultraviolet rays to be cured layer by layer and laminated, and photocuring from a material jet nozzle.
- a material jet method injetography in which a cured layer having a predetermined shape is laminated to produce a three-dimensional model by discharging the sex resin composition and immediately irradiating it with light such as ultraviolet rays to cure the resin composition.
- a stereolithography method (hereinafter, also referred to as "material jet stereolithography method") by a method) is known.
- the material jet stereolithography method is widely attracting attention as a modeling method that can be realized by a small modeling device (3D printer) that can freely produce a three-dimensional model based on CAD (Computer Aided Design) data.
- CAD Computer Aided Design
- Patent Document 1 describes a monofunctional ethylenically unsaturated monomer (A) having no urethane group and a polyfunctional composition having no urethane group.
- a model material composition is disclosed in which each of the homopolymers of the above has a predetermined glass transition temperature.
- a photocured product of a resin composition for stereolithography used in a stereolithography method is, for example, an electron It is expected to be used as a member for printed circuit boards of equipment in a high temperature environment exceeding 100 ° C.
- model material a material jet stereolithography method
- a method for improving the heat resistance of a model material has been proposed, but the heat resistance in a harsher temperature environment is not always sufficient. ..
- the present invention provides a resin composition for stereolithography which has high heat resistance, is less likely to cause thermal expansion even in a high temperature environment, and can form a photocurable product capable of maintaining high dimensional stability. With the goal.
- the present inventors have completed the present invention as a result of diligent studies to solve the above problems.
- a resin composition for stereolithography Contains polymerizable compounds
- the polymerizable compound is At least one polyfunctional ethylenically unsaturated monomer (B) having a ring structure other than the isocyanurate ring structure; and at least one polyfunctional ethylenically unsaturated monomer (C) having an isocyanurate ring structure.
- the content of the monomer (C) is 5 to 80 parts by mass with respect to 100 parts by mass of the resin composition for stereolithography, and the content of the monofunctional ethylenically unsaturated monomer (A) is ,
- the resin composition for stereolithography which is less than 70 parts by mass with respect to 100 parts by mass of the resin composition for stereolithography.
- the resin composition for stereolithography according to [1] wherein the polymerizable compound further contains at least one monofunctional ethylenically unsaturated monomer (A).
- At least one polyfunctional ethylenically unsaturated monomer (B) having a ring structure other than the isocyanurate ring structure is a polyfunctional ethylenically unsaturated monomer having an alicyclic structure.
- the polyfunctional ethylenically unsaturated monomer (B) having a ring structure other than the isocyanurate ring structure has a linear expansion coefficient of 200 ppm measured below the glass transition temperature of the homopolymer according to JIS K 7197.
- the polyfunctional ethylenically unsaturated monomer (C) having an isocyanurate ring structure has a linear expansion coefficient of 200 ppm or less as measured below the glass transition temperature of the homopolymer according to JIS K 7197.
- a resin composition for stereolithography capable of forming a photocured product having high heat resistance, less likely to cause thermal expansion even in a high temperature environment, and maintaining high dimensional stability by the stereolithography method.
- a product and a photocurable product thereof can be provided.
- the resin composition for photoforming of the present invention is a composition used in a stereolithography method, and constitutes a photocured product by photocuring.
- the stereolithography method includes a method by a liquid tank photopolymerization method (SLA, DLP, LCD), a material jet method (MJM), or the like.
- the "resin composition for stereolithography” means the composition used in the stereolithography method
- the "photocured product” means the photocured product of the resin composition for stereolithography.
- the description of each composition, characteristics, etc. regarding the stereolithography resin composition is also applied to the model material composition used in the material jet stereolithography method, unless otherwise specified.
- the description of each composition, characteristics, etc. relating to the photocured product in the present specification also applies to the model material which is the photocured product of the model material composition, unless otherwise specified.
- the resin composition for photoforming of the present invention contains a polymerizable compound, and the polymerizable compound has at least one polyfunctional ethylenically unsaturated monomer (B) having a ring structure other than the isocyanurate ring structure.
- B polyfunctional ethylenically unsaturated monomer
- C polyfunctional ethylenically unsaturated monomer having an isocyanurate ring structure
- the ethylenically unsaturated monomer is a polymerizable monomer having at least one ethylenically double bond in the molecule having a property of being cured by energy rays.
- the monofunctional ethylenically unsaturated monomer is a polymerizable monomer having one ethylenically double bond in the molecule, and the polyfunctional ethylenically unsaturated monomer has two ethylenically double bonds in the molecule. It is a polymerizable monomer having more than one.
- the resin composition for stereolithography of the present invention can easily suppress an excessive increase in viscosity of the resin composition for stereolithography, and enhances the dimensional stability of the obtained photocured product.
- Cheap In particular, by including the monomer B in combination with the monomer C described later, it is easy to suppress the thermal expansion of the obtained photocured product in a high temperature environment and improve the dimensional stability.
- Examples of the monomer B include a polyfunctional ethylenically unsaturated monomer having an alicyclic structure or an aromatic hydrocarbon ring structure. These monomers may be used alone or in combination of two or more.
- the alicyclic structure refers to an aliphatic cyclic structure in which carbon atoms are cyclically bonded.
- Examples of the polyfunctional ethylenically unsaturated monomer having an alicyclic structure include a polyfunctional (meth) acrylate having an alicyclic structure.
- Examples of the polyfunctional (meth) acrylate having an alicyclic structure include di or tri (meth) acrylate having an alicyclic structure, and specifically, cyclohexanedimethanol di (meth) acrylate and tricyclodecandy. Examples thereof include methanol di (meth) acrylate.
- "(meth) acrylate” represents an acrylate and / or a methacrylate.
- polyfunctional ethylenically unsaturated monomer having an aromatic hydrocarbon ring structure examples include bisphenol A ethylene oxide adduct di (meth) acrylate and bisphenol A propylene oxide adduct di (meth) acrylate.
- a polyfunctional ethylenically unsaturated monomer having an alicyclic structure is preferable from the viewpoint of dimensional stability.
- the polyfunctional ethylenically unsaturated monomer having a preferable alicyclic structure is a di or tri (meth) acrylate having an alicyclic structure, and more preferably a di (meth) having a cyclic structure having 5 to 30 carbon atoms.
- Acrylate or tri (meth) acrylate more preferably a di or tri (meth) acrylate having an alicyclic structure of 6 to 20 carbon atoms, particularly preferably a di or tri (meth) acrylate having an alicyclic structure of 8 to 15 carbon atoms. It is a (meth) acrylate.
- the monomer B is a polyfunctional ethylenically unsaturated monomer having an alicyclic structure, it is difficult to thermally expand and can form a photocured product having high dimensional stability even in a high temperature environment. It is easy to obtain a resin composition for modeling. Further, it is easier to suppress an excessive increase in the viscosity of the stereolithography resin composition than when the monomer B is a polyfunctional ethylenically unsaturated monomer having an aromatic hydrocarbon ring.
- the linear expansion coefficient of the homopolymer of the monomer B is preferably 200 ppm or less.
- the coefficient of linear expansion is more preferably 150 ppm or less, further preferably 130 ppm or less, particularly preferably 120 ppm or less, and particularly preferably 100 ppm or less.
- the lower the coefficient of linear expansion the higher the effect of suppressing thermal expansion tends to be. Therefore, the lower limit is not particularly limited and may be 0 ppm.
- the coefficient of linear expansion is not more than the above upper limit value, the thermal expansion of the photocured product obtained from the stereolithography resin composition in a high temperature environment is suppressed, and the dimensional stability of the photocured product is likely to be improved.
- the coefficient of linear expansion is measured in a temperature range below the glass transition temperature, for example, from room temperature to the glass transition temperature of the homopolymer in the range of -30 ° C, according to JIS K 7197, using a homopolymer of monomer B as a test piece. it can. Specifically, for example, it can be measured by the method described in Examples. For example, for a homopolymer of monomer B, a photopolymerization initiator is added to monomer B, and then an integrated light amount of 500 mJ / cm is measured by a metal halide lamp. It is obtained by irradiating and curing the ultraviolet rays of 2.
- the content of the monomer B is preferably 5 to 65 parts by mass with respect to 100 parts by mass of the stereolithography resin composition.
- the content of the monomer B is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, still more preferably 15 parts by mass or more, based on 100 parts by mass of the stereolithography resin composition from the viewpoint of dimensional stability. It is 20 parts by mass or more. Further, from the viewpoint of the viscosity of the stereolithography resin composition, it is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, and further preferably 45 parts by mass or less.
- the content of the monomer B suitable for the material jet stereolithography method is determined. It is 5 to 50 parts by mass with respect to 100 parts by mass of the model material composition. If the content of the monomer B is less than the above lower limit value, it is difficult to impart sufficiently high dimensional stability to the obtained model material, and if it exceeds the above upper limit value, the viscosity of the model material composition increases excessively. It's easy to do.
- the content of the monomer B is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and further preferably 20 parts by mass with respect to 100 parts by mass of the model material composition. It is more than a part. Further, from the viewpoint of the viscosity of the model material composition, it is preferably 45 parts by mass or less, more preferably 35 parts by mass or less, and further preferably 30 parts by mass or less.
- the monomer C is not particularly limited as long as it is a polyfunctional ethylenically unsaturated monomer having an isocyanurate ring structure, and for example, a polyfunctional (meth) acrylate having an isocyanurate ring structure or an isocyanurate ring structure can be used. Examples thereof include allyl compounds having. These monomers may be used alone or in combination of two or more.
- Examples of the polyfunctional (meth) acrylate having an isocyanurate ring structure include isocyanurate ethylene oxide-modified di or triacrylate, ethoxylated isocyanurate triacrylate, tris (2-hydroxyethyl) isocyanurate triacrylate, and bis (2-hydroxyethyl).
- Examples of the allyl compound having an isocyanurate ring structure include triallyl isocyanurate and diallyl isocyanurate.
- a polyfunctional (meth) acrylate having an isocyanurate ring structure is preferable, and a tri (meth) acrylate having an isocyanurate ring structure is particularly preferable. Is a tris (2-hydroxyethyl) isocyanurate triacrylate.
- the linear expansion coefficient of the homopolymer of the monomer C is preferably 200 ppm or less.
- the coefficient of linear expansion is more preferably 150 ppm or less, further preferably 120 ppm or less, particularly preferably 100 ppm or less, and particularly preferably 80 ppm or less.
- the lower the coefficient of linear expansion the higher the effect of suppressing thermal expansion tends to be. Therefore, the lower limit is not particularly limited and may be 0 ppm.
- the coefficient of linear expansion is not more than the above upper limit value, it is easy to suppress the thermal expansion of the photocured product obtained from the stereolithography resin composition, and it is easy to improve the dimensional stability of the photocured product in a high temperature environment.
- the coefficient of linear expansion is measured in a temperature range below the glass transition temperature, for example, from room temperature to the glass transition temperature of the homopolymer in the range of -30 ° C, according to JIS K 7197, using a homopolymer of monomer C as a test piece. it can. Specifically, for example, it can be measured by the method described in Examples. For example, for a homopolymer of monomer C, a photopolymerization initiator is added to monomer C, and then an integrated light amount of 500 mJ / cm is measured by a metal halide lamp. It is obtained by irradiating and curing the ultraviolet rays of 2.
- the content of the monomer C is 5 to 80 parts by mass with respect to 100 parts by mass of the stereolithography resin composition. If the content of the monomer C is less than the above lower limit, it is difficult to impart sufficiently high dimensional stability to the obtained photocured product, and if it exceeds the above upper limit, the viscosity of the stereolithography resin composition is exceeded. Is likely to rise excessively.
- the content of the monomer C is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, still more preferably 15 parts by mass or more, based on 100 parts by mass of the stereolithography resin composition from the viewpoint of dimensional stability. It is 20 parts by mass or more. Further, from the viewpoint of the viscosity of the stereolithography resin composition, it is preferably 75 parts by mass or less, more preferably 70 parts by mass or less, and further preferably 60 parts by mass or less.
- the content of the monomer C suitable for the material jet stereolithography method is determined. It is 5 to 50 parts by mass with respect to 100 parts by mass of the model material composition. If the content of the monomer C is less than the above lower limit value, it is difficult to impart sufficiently high dimensional stability to the obtained model material, and if it exceeds the above upper limit value, the viscosity of the model material composition becomes excessive. It rises easily and is difficult to apply to the material jet stereolithography method.
- the content of the monomer C is preferably 10 parts by mass or more, more preferably 15 parts by mass or more, and further preferably 20 parts by mass with respect to 100 parts by mass of the model material composition. It is more than a part. Further, from the viewpoint of the viscosity of the model material composition, it is preferably 40 parts by mass or less, more preferably 35 parts by mass or less, and further preferably 30 parts by mass or less.
- the ratio of the total mass of the monomer B to the total mass of the monomer C, and the monomer B: monomer C are preferably 1:20. It is ⁇ 10: 1, more preferably 1:10 to 5: 1, still more preferably 1: 5 to 2: 1, and particularly preferably 1: 1.2 to 1.2: 1.
- mass ratio of the monomer B and the monomer C is within the above range, it is easy to impart excellent dimensional stability to the obtained photocured product.
- the resin composition for stereolithography contains the monomer B and the monomer C in the same mass ratio, it is easy to suppress the vibration of the molecules in the obtained photocured product, and the dimensional stability is further improved. Cheap.
- the stereolithography resin composition when the stereolithography resin composition is a model material composition used in the material jet stereolithography method, the total mass and unit amount of the monomer B suitable for the material jet stereolithography method.
- the ratio of body C to the total mass, monomer B: monomer C is preferably 1:10 to 10: 1, more preferably 1: 5 to 5: 1, and even more preferably 1: 1. It is 2 to 2: 1, particularly preferably 1: 1.2 to 1.2: 1.
- the mass ratio of the monomer B and the monomer C is within the above range, it is easy to impart excellent dimensional stability to the obtained model material.
- the model material composition contains the monomer B and the monomer C in the same mass ratio, it is easy to suppress the vibration of the molecules in the obtained model material, and it is easy to improve the dimensional stability.
- the resin composition for stereolithography of the present invention is monofunctional ethylenically unsaturated in addition to the monomer B and the monomer C from the viewpoint that the viscosity can be easily adjusted to an appropriate level according to the stereolithography method to be adopted. It is preferable to contain the monomer (A) (hereinafter, also referred to as “monomer A”). When the resin composition for stereolithography of the present invention contains monomer A, it is easy to adjust the viscosity to be suitable for the material jet stereolithography method.
- the monofunctional ethylenically unsaturated monomer (A) is an alkyl (meth) acrylate having a linear or branched alkyl group; an alicyclic structure, an aromatic ring structure or an aromatic ring structure in the molecule.
- examples thereof include (meth) acrylates having a ring structure such as a heterocyclic structure; and monofunctional ethylenically unsaturated monomers containing nitrogen atoms such as (meth) acrylamide and N-vinyllactams. These monomers may be used alone or in combination of two or more.
- "(meth) acrylamide” represents acrylamide and / or methacrylamide.
- the aromatic ring structure refers to an aromatic cyclic structure in which carbon atoms are cyclically bonded
- the heterocyclic structure refers to a structure in which a carbon atom and one or more heteroatoms are cyclically bonded.
- alkyl (meth) acrylate having a linear or branched alkyl group examples include a linear or branched alkyl group having preferably 4 to 30 carbon atoms, more preferably 6 to 20 carbon atoms.
- Alkyl (meth) acrylate having is mentioned. Specifically, for example, methyl (meth) acrylate, ethyl (meth) acrylate, isobutyl (meth) acrylate, amyl (meth) acrylate, isoamyl (meth) acrylate, octyl (meth) acrylate, isooctyl (meth) acrylate, decyl.
- Examples of the (meth) acrylate having an alicyclic structure include (meth) acrylate having an alicyclic structure preferably having 6 to 20 carbon atoms and more preferably 8 to 15 carbon atoms.
- cyclohexyl (meth) acrylate, 4-t-butylcyclohexyl (meth) acrylate, isobornyl (meth) acrylate, dicyclopentanyl (meth) acrylate, adamantyl (meth) acrylate, 3,3,5 -Trimethylcyclohexanol (meth) acrylate and the like can be mentioned.
- Examples of the (meth) acrylate having an aromatic ring structure include (meth) acrylate having an aromatic ring structure having preferably 6 to 20 carbon atoms and more preferably 8 to 15 carbon atoms. Specifically, for example, phenoxyethyl (meth) acrylate, phenoxy-polyethylene glycol (meth) acrylate, 2-hydroxy-3-phenoxypropyl (meth) acrylate, nonylphenol ethylene oxide adduct (meth) acrylate, 2- (meth).
- Examples of the (meth) acrylate having a heterocyclic structure include (meth) acrylate having a heterocyclic structure having preferably 5 to 20 carbon atoms and more preferably 7 to 15 carbon atoms.
- tetrahydrofurfuryl (meth) acrylate, cyclic trimethylolpropane formal (meth) acrylate, 4- (meth) acryloyloxymethyl-2-methyl-2-ethyl-1,3-dioxolane, 4 -(Meta) acryloyloxymethyl-2-cyclohexyl-1,3-dioxolane and the like can be mentioned.
- examples of the monofunctional ethylenically unsaturated monomer containing a nitrogen atom, which is different from the above (meth) acrylate include (meth) acrylamide [for example, N, N-dimethylacrylamide, N, N-diethylacrylamide]. , N-isopropylacrylamide, hydroxyethylacrylamide, hydroxypropylacrylamide, N, N-acryloylmorpholin, etc.], N-vinyllactams (eg, N-vinylpyrrolidone, N-vinylcaprolactam, etc.), N-vinylformamide, etc. Be done.
- acrylamide for example, N, N-dimethylacrylamide, N, N-diethylacrylamide.
- N-vinyllactams eg, N-vinylpyrrol
- the monomer A is preferably a monofunctional ethylenically unsaturated monomer having a ring structure in the molecule.
- the monomer A is a monofunctional ethylenically unsaturated monomer having a ring structure in the molecule, it becomes easy to obtain a photocured product having high dimensional stability. It is presumed that this is because it becomes easier to suppress the vibration of the molecules in the photocured product obtained from the stereolithography resin composition as compared with the monomer A having no ring structure.
- the content of the monofunctional ethylenically unsaturated monomer having a ring structure in the molecule is based on the total mass of the monofunctional ethylenically unsaturated monomer (A). , Preferably 50% by mass or more, more preferably 80% by mass or more, and all monofunctional ethylenically unsaturated monomers (A) contained in the resin composition for photoforming have a ring structure in the molecule. It may have.
- the homopolymer glass transition temperature Tg of the monomer A is preferably 80 ° C. or higher, more preferably 100 ° C. or higher, and further preferably 120 ° C. or higher.
- the glass transition temperature Tg of the monomer A is preferably 200 ° C. or lower, more preferably 180 ° C. or lower, still more preferably 160 ° C. or lower, from the viewpoint of curing shrinkage when the stereolithography resin composition is cured.
- the glass transition temperature is measured by a differential scanning calorimeter (DSC) using a homopolymer of monomer A as a test piece. Specifically, for example, it is measured by the method described in Examples.
- the content of the monomer A is less than 70 parts by mass with respect to 100 parts by mass of the stereolithography resin composition.
- the lower limit of the content of the monomer A is not particularly limited, but from the viewpoint of imparting a viscosity suitable for the stereolithography method to the stereolithography resin composition, with respect to 100 parts by mass of the stereolithography resin composition. It is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 19 parts by mass or more. From the viewpoint of dimensional stability, it is preferably 65 parts by mass or less, more preferably 59 parts by mass or less, further preferably 55 parts by mass or less, still more preferably 53 parts by mass or less, and particularly preferably 48 parts by mass or less.
- the stereolithography resin composition when the stereolithography resin composition is a model material composition used in the material jet stereolithography method, the model material composition is added to the monomer B and the monomer C. And contains monomer A.
- the content of the monomer A suitable for the material jet stereolithography method is 19 to 59 parts by mass with respect to 100 parts by mass of the model material composition. If the content of the monomer A is less than the above lower limit value, it is difficult to adjust the viscosity of the model material composition to an appropriate range, and if it exceeds the above upper limit value, the dimensional stability is sufficiently high for the obtained model material. It becomes difficult to give sex.
- the content of the monomer A is preferably 25 parts by mass or more with respect to 100 parts by mass of the model material composition from the viewpoint of imparting a viscosity suitable for the material jet stereolithography to the model material composition. , More preferably 30 parts by mass or more, still more preferably 35 parts by mass or more. From the viewpoint of dimensional stability, it is preferably 55 parts by mass or less, more preferably 53 parts by mass or less, and further preferably 48 parts by mass or less.
- the optical modeling resin composition of the present invention contains monomer A
- the ratio of the total mass of the monomer A to the total mass of the monomer B in the optical modeling resin composition is preferably 10: 1 to 1: 8, more preferably 5: 1 to 1: 4, and even more preferably 2: 1 to 1: 2.
- the mass ratio of the monomer A and the monomer B is within the above range, both the appropriate viscosity of the stereolithography resin composition and the high dimensional stability of the obtained photocured product in a high temperature environment are achieved. It's easy to do.
- the resin composition for stereolithography is a model material composition used in the material jet stereolithography method
- the total mass and simple mass of the monomer A suitable for the material jet stereolithography method are preferably 10: 1 to 1: 3, more preferably 5: 1 to 1: 2, and even more preferably 2. 1: 1 to 1: 1.
- the mass ratio of the monomer A and the monomer B is within the above range, it is easy to achieve both an appropriate viscosity of the model material composition and high dimensional stability of the obtained model material in a high temperature environment.
- the ratio of the total mass of the monomer A to the total mass of the monomer C in the optical modeling resin composition is preferably 10: 1 to 1:10, more preferably 5: 1 to 1: 5, and even more preferably 2: 1 to 1: 2.
- the mass ratio of the monomer A and the monomer C is within the above range, both the appropriate viscosity of the stereolithography resin composition and the high dimensional stability of the obtained photocured product in a high temperature environment are achieved. It's easy to do.
- the resin composition for stereolithography is a model material composition used in the material jet stereolithography method
- the total mass and the single amount of the monomer A suitable for the material jet stereolithography method is preferably 10: 1 to 1: 3, more preferably 5: 1 to 1: 2, and even more preferably 2: 1. It is 1 to 1: 1.
- the mass ratio of the monomer A and the monomer C is within the above range, it is easy to achieve both an appropriate viscosity of the model material composition and high dimensional stability of the obtained model material in a high temperature environment.
- the resin composition for stereolithography of the present invention suppresses the thermal expansion of the obtained photocured product and sufficiently provides dimensional stability in a high temperature environment. Easy to improve.
- the photomodeling resin composition of the present invention contains monomer A, the ratio of the total mass of the monomer B and the monomer C to the total mass of the monomer A in the photomodeling resin composition.
- the (monomer B + monomer C) / monomer A (mass ratio) is preferably 0.5 to 10, more preferably 0.5 to 5, still more preferably 0.8 to 4, and even more preferably. Is 0.8 to 3, particularly preferably 1 to 2, and particularly preferably 1 to 1.5.
- the total content of the monomer B and the monomer C is the total of all the polymerizable compounds in the stereolithography resin composition from the viewpoint of dimensional stability. It is preferably 30% by mass or more, more preferably 35% by mass or more, and further preferably 40% by mass or more with respect to the total amount.
- the viscosity of the stereolithography resin composition it is preferably 95% by mass or less, more preferably 80% by mass or less, still more preferably 70% by mass or less, and particularly preferably 60% by mass or less.
- a "polymerizable compound” represents a compound having a polymerizable group such as a polymerizable monomer and a polymerizable oligomer.
- the total content of the monomer B and the monomer C is preferable with respect to 100 parts by mass of the stereolithography resin composition from the viewpoint of dimensional stability.
- the resin composition for stereolithography of the present invention may contain monomer B and monomer C, and optionally other polymerizable compounds other than monomer A.
- examples of other polymerizable compounds include polyfunctional polymerizable monomers having no ring structure and polymerizable oligomers.
- the "polymerizable oligomer” is a photocurable component having a property of being cured by energy rays, and has a weight average molecular weight Mw of 1,000 to 10,000. The weight average molecular weight Mw is measured in terms of standard polystyrene using GPC (Gel Permeation Chromatography).
- polyfunctional polymerizable monomer having no ring structure examples include epoxy poly (meth) acrylate, polyester poly (meth) acrylate, and urethane as a polyfunctional ethylenically unsaturated monomer having no ring structure in the molecule.
- examples include poly (meth) acrylate having a group. These polyfunctional polymerizable monomers may be used alone or in combination of two or more.
- polymerizable oligomer examples include an epoxy (meth) acrylate oligomer, a polyester (meth) acrylate oligomer, and a urethane (meth) acrylate oligomer. These polymerizable oligomers may be used alone or in combination of two or more. By containing the polymerizable oligomer, it becomes easy to impart flexibility to the photocured product obtained from the stereolithography resin composition.
- the preferred polymerizable oligomer is a polymerizable oligomer having a urethane group, and more preferably a urethane (meth) acrylate oligomer.
- the stereolithography resin composition contains other polymerizable compounds
- the content thereof is not limited as long as it does not impair the effects of the present invention.
- 100 parts by mass of the stereolithography resin composition It is preferably 0.1 to 30 parts by mass, more preferably 0.5 to 15 parts by mass, and further preferably 1 to 10 parts by mass.
- the total amount of the polymerizable compound contained in the stereolithography resin composition is preferably 10 to 99 parts by mass, more preferably 29 to 99 parts by mass, and further preferably more preferably 29 to 99 parts by mass with respect to 100 parts by mass of the stereolithography resin composition. It is 50 to 98 parts by mass, particularly preferably 80 to 95 parts by mass.
- the resin composition for stereolithography of the present invention may contain other additives, if necessary, as long as the effects of the present invention are not impaired.
- Other additives include, for example, photopolymerization initiators, surface modifiers, colorants, storage stabilizers, antioxidants, UV absorbers, light stabilizers, polymerization inhibitors, chain transfer agents, fillers, dilutions. Examples include solvents and thickeners.
- the photopolymerization initiator is not particularly limited as long as it is a compound that promotes a radical reaction by irradiating light having a wavelength in the ultraviolet, near-ultraviolet, or visible light region.
- the photopolymerization initiator include benzoin compounds having 14 to 18 carbon atoms [for example, benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isobutyl ether, etc.], and acetophenone compounds having 8 to 18 carbon atoms [for example.
- Thioxanthone compounds for example, 2,4-diethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, etc.] ketal compounds having 16 to 17 carbon atoms [for example, acetophenone dimethyl ketal, benzyl dimethyl ketal, etc.], 13 to 13 carbon atoms.
- benzophenone compounds eg, benzophenone, 4-benzoyl-4'-methyldiphenylsulfide, 4,4'-bismethylaminobenzophenone, etc.
- acylphosphine oxide compounds having 22-28 carbon atoms [eg, 2,4.
- 6-trimethylbenzoyl-diphenyl-phosphine oxide bis- (2,6-dimethoxybenzoyl) -2,4,4-trimethylpentylphosphine oxide, bis (2,4,6-trimethylbenzoyl) -phenylphosphine oxide ], ⁇ -Aminoalkylphenone compound [for example, 2-methyl-1 [4- (methylthio) phenyl] -2-morpholinopropane-1-one, 2-benzyl-2-dimethylamino-1- (4-morpholinophenyl) ) Butanone-1,2-methyl-1- [4- (methoxythio) -phenyl] -2-morpholinopropane-2-one, 2-dimethylamino-2- (4-methyl-benzyl) -1- (4-) Morifolin-4-yl-phenyl) -butane-1-one, etc.], a mixture of these compounds, and the like.
- the photo-cured product and the photo-shaped product obtained by photo-curing the resin composition for stereolithography are less likely to yellow, and the obtained photo-cured product and the photo-shaped product have high light resistance over time.
- 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide is preferable because it does not easily turn yellow.
- Examples of available acylphosphine oxide compounds include DAROCURE TPO manufactured by BASF.
- the stereolithography resin composition contains a photopolymerization initiator
- the content thereof is preferably 1 to 15 parts by mass, more preferably 3 parts by mass or more, based on 100 parts by mass of the stereolithography resin composition. It is more preferably 12 parts by mass or less.
- the content of the photopolymerization initiator is at least the above lower limit value, the amount of the unreacted polymerization component can be sufficiently reduced, and the curability of the photocurable product can be sufficiently enhanced.
- the content of the photopolymerization initiator is not more than the above upper limit value, it is easy to reduce the amount of the photopolymerization initiator remaining unreacted in the photocured product, and the unreacted photopolymerization initiator remains. It is easy to suppress the yellowing of the photocured product caused by the above.
- the surface conditioner is a component that adjusts the surface tension of the stereolithography resin composition within an appropriate range, and the type thereof is not particularly limited.
- the ejection property can be stabilized and the model material composition can be stabilized when the stereolithography resin composition is used in the material jet stereolithography method.
- Interfacial mixing between the product and the support material composition can be suppressed. As a result, it is easy to obtain a stereolithographic object with good dimensional accuracy.
- Examples of the surface conditioner include silicone compounds.
- Examples of the silicone-based compound include a silicone-based compound having a polydimethylsiloxane structure. Specific examples thereof include polyether-modified polydimethylsiloxane, polyester-modified polydimethylsiloxane, and polyaralkyl-modified polydimethylsiloxane.
- a surface conditioner other than the silicone compound for example, a fluorine-based surface conditioner
- these may be used alone or in combination of two or more.
- the stereolithography resin composition contains a surface conditioner
- the content thereof is preferably 0.005 to 3 parts by mass, more preferably 0.01 with respect to 100 parts by mass of the stereolithography resin composition. It is 5 parts by mass or more, and more preferably 1.5 parts by mass or less.
- the content of the surface conditioner is within the above range, it is easy to adjust the surface tension of the stereolithography resin composition to an appropriate range.
- the storage stabilizer is a component that can enhance the storage stability of the stereolithography resin composition. Further, in the case of a model material composition in which the stereolithography resin composition is used in the material jet stereolithography method, it is possible to prevent head clogging caused by polymerization of the polymerizable compound by thermal energy.
- Examples of the storage stabilizer include hindered amine compounds (HALS), phenolic antioxidants, phosphorus-based antioxidants, and the like. Specifically, hydroquinone, methquinone, benzoquinone, p-methoxyphenol, hydroquinone monomethyl ether, hydroquinone monobutyl ether, TEMPO, 4-hydroxy-TEMPO, TEMPOL, H-TEMPO (4-hydroxy-2,2,6,6- Tetramethylpiperidin-N-oxyl), TEMPO Al; IRGASTAB UV-10, IRGASTAB UV-22, FIRSTCURE ST-1; t-butylcatechol, pyrogallol; BASF TINUVIN 111 FDL, TINUVIN 144, TINUVIN 292, TINUVIN XP40, TINUVIN XP60, TINUVIN 400 and the like can be mentioned. These may be used alone or in combination of two or more.
- HALS hindered amine compounds
- phenolic antioxidants phenolic antioxidants
- the stereolithography resin composition contains a storage stabilizer
- the content thereof is preferably 0.05 to 3 parts by mass with respect to 100 parts by mass of the stereolithography resin composition from the viewpoint of easily obtaining the above effect. Yes, more preferably 0.08 parts by mass or more, and more preferably 2 parts by mass or less.
- the resin composition for stereolithography of the present invention may further contain a colorant.
- the colorant is not particularly limited, but since the resin composition for stereolithography of the present invention is non-aqueous, pigments that are easily dispersed uniformly in a water-insoluble medium and dyes that are easily dissolved are preferable.
- an inorganic pigment or an organic pigment can be used.
- inorganic pigments include titanium oxide, zinc oxide, zinc oxide, lithopone, iron oxide, aluminum oxide, silicon dioxide, kaolinite, montmorillonite, talc, barium sulfate, calcium carbonate, silica, alumina, cadmium red, red pepper, molybdenum.
- organic pigments examples include azo-based, azomethine-based, polyazo-based, phthalocyanine-based, quinacridone-based, anthraquinone-based, indigo-based, thioindigo-based, quinophthalone-based, benzimidazolone-based, and isoindoline-based organic pigments.
- carbon black composed of acidic, neutral or basic carbon may be used.
- hollow particles of crosslinked acrylic resin may be used as the organic pigment.
- pigments of three primary colors of black, cyan, magenta, and yellow are usually used, but pigments having other hues and metallic glossy pigments such as gold and silver are used.
- Colorless or light-colored extender pigments and the like can also be used depending on the purpose.
- the above colorants may be used alone or in combination of two or more. Further, in the present invention, two or more kinds of organic pigments or solid solutions of organic pigments can be used in combination. Further, different colorants may be used for each of the droplets and the liquid to be dropped, or the same colorant may be used.
- Dispersion of the colorant includes, for example, bead mill, ball mill, sand mill, attritor, roll mill, jet mill, homogenizer, paint shaker, kneader, agitator, henschel mixer, colloid mill, ultrasonic homogenizer, pearl mill, wet jet mill and the like.
- the device can be used, or a mixer such as a line mixer may be used.
- the classification treatment may be performed using a centrifuge, a filter, a cross flow, or the like for the purpose of removing the coarse particles of the colorant.
- a dispersant When dispersing the above colorant, a dispersant may be added.
- the type of dispersant is not particularly limited, but it is preferable to use a known polymer dispersant.
- the content of the dispersant is appropriately selected depending on the purpose of use, and may be, for example, 0.01 to 5 parts by mass with respect to 100 parts by mass of the stereolithography resin composition.
- a sinagist suitable for various colorants may be used as a dispersion aid.
- the content of the colorant is appropriately selected depending on the color and the purpose of use, but from the viewpoint of image density and storage stability, it is preferably 0.05 to 30 with respect to 100 parts by mass of the stereolithography resin composition. It is by mass, more preferably 0.1 to 10 parts by mass.
- the method for producing the stereolithography resin composition of the present invention is not particularly limited. For example, it can be produced by uniformly mixing the components constituting the stereolithography resin composition using a mixing and stirring device or the like.
- the viscosity of the resin composition for stereolithography of the present invention may have a viscosity suitable for the stereolithography method according to the stereolithography method to be adopted, and is preferably 10 to 2500 mPa ⁇ s at 25 ° C. May be 20 to 1500 mPa ⁇ s.
- the viscosity of the model material composition of the present invention is the ejection property from the material jet nozzle.
- the viscosity measurement can be performed using an R100 type viscometer in accordance with JIS Z 8803.
- the viscosity of the stereolithography resin composition can be controlled by adjusting the type of ethylenically unsaturated monomer and its blending ratio, the type of diluting solvent and thickener, and the amount of the thickener added thereto.
- the coefficient of linear expansion of the photocured product of the present invention obtained by photocuring the resin composition for stereolithography of the present invention is preferably 150 ppm or less.
- the coefficient of linear expansion is more preferably 130 ppm or less, still more preferably 120 pm or less, and particularly preferably less than 100 ppm.
- the lower the coefficient of linear expansion the higher the effect of suppressing thermal expansion tends to be. Therefore, the lower limit is not particularly limited and may be 0 ppm.
- the coefficient of linear expansion is not more than the above upper limit value, for example, even in a high temperature environment exceeding 100 ° C., it is easy to suppress the thermal expansion of the photocured product, and high dimensional stability can be ensured.
- the coefficient of linear expansion is measured, for example, according to JIS K 7197, in a temperature range below the glass transition temperature, for example, from room temperature to the glass transition temperature of the homopolymer ⁇ 30 ° C.
- a photocured product obtained by irradiating a resin composition for stereolithography with ultraviolet rays so that the total irradiation light amount is 500 mJ / cm 2 and curing it is used as a test piece, and measurement is performed by the method described in Examples. Will be done.
- the total irradiation light amount is measured by, for example, UV METER UVPF-36 (manufactured by Eye Graphics Co., Ltd.).
- the photocured product of the present invention has a low coefficient of linear expansion and a small dimensional change in a high temperature environment, and is therefore suitable for use in a high temperature environment.
- Examples of such an application include a housing of an electronic device and a member constituting the electronic device.
- the photocurable product of the present invention is suitable for a member for a printed circuit board of an electronic device (for example, an insulating plate for printed wiring).
- a printed circuit board member is subjected to a step of forming a metal wiring by linearly arranging a liquid metal on the printed circuit board member and firing it when the printed circuit board is manufactured. Such a step is usually performed in a high temperature environment exceeding 100 ° C.
- the printed circuit board member When the printed circuit board member is composed of a photocurable material that does not have sufficient heat resistance, it tends to expand thermally in such a high temperature environment, and a tensile stress is applied to the metal wire arranged on the member. By giving, there is a possibility that the metal wire may be cracked.
- the printed circuit board member formed by using the photocurable product of the present invention does not easily expand thermally even in such a high temperature environment and has high dimensional stability. Is unlikely to occur.
- the printed circuit board member can be manufactured by molding the printed circuit board member into a desired shape by a stereolithography method using the resin composition for photoforming of the present invention and photocuring the member. For example, it can be produced by forming an optical model (or a three-dimensional model) having a desired shape of a printed circuit board member by a material jet stereolithography method using the model material composition of the present invention. The stereolithography may be produced, for example, by the method described later.
- the model material composition of the present invention is preferably used in combination with a support material for supporting the model material during three-dimensional modeling in order to form a complicated shape or a precise shape with high accuracy. Therefore, the present invention includes a model material composition of the present invention and a material jet stereolithography including a support material composition for forming a support material by the material jet stereolithography method used together with the model material composition. Composition sets for use are also included.
- the support material composition is a composition used in the material jet stereolithography method, and constitutes a support material by photocuring. After producing the model material, the support material can be removed from the model material by physically peeling the support material from the model material or by dissolving the support material in an organic solvent or water.
- the model material composition of the present invention can be used in combination with various conventionally known compositions as a support material composition, but the model material is not damaged when the support material is removed, and is environmentally friendly. Since the support material can be removed cleanly and easily in detail, the support material composition constituting the material jet stereolithography composition set of the present invention is preferably water-soluble.
- Examples of the water-soluble support material composition include those containing a polyalkylene glycol containing an oxybutylene group.
- the polyalkylene glycol containing an oxybutylene group is water-soluble, it does not have enough hydrophilicity to reduce the supporting force of the supporting material when the supporting material is formed.
- the polyalkylene glycol containing an oxybutylene group is water-soluble, it is excellent in water removal property of the support material when the support material is formed.
- Polyalkylene glycol containing an oxybutylene group is a water-soluble resin for imparting appropriate hydrophilicity to a support material, and by adding this, a support material having both water removability and support power can be obtained. Can be done.
- the polyalkylene glycol containing an oxybutylene group is not particularly limited in the structure of the alkylene portion as long as it contains an oxybutylene group, and is, for example, a polybutylene glycol having only an oxybutylene group (oxytetramethylene group). Alternatively, it may be a polybutylene polyoxyalkylene glycol having both an oxybutylene group and another oxyalkylene group (for example, polybutylene polyethylene glycol).
- Polybutylene glycol is represented by the following chemical formula (1), and polybutylene polyethylene glycol is represented by the following chemical formula (2).
- n is preferably an integer of 2 to 150. More preferably, m is 6 to 200 and n is 3 to 100. Further, the oxybutylene group in the chemical formula (1) and the chemical formula (2) may be linear or branched.
- the content of the polyalkylene glycol containing an oxybutylene group is preferably 15 to 75 parts by mass, more preferably 17 to 72 parts by mass, and further preferably 20 to 70 parts by mass with respect to 100 parts by mass of the support material composition. is there.
- the content is at least the above lower limit value, the hydrophilicity of the support material is improved, and the water removability of the support material is likely to be improved.
- the content is not more than the above upper limit value, the softening of the support material is suppressed and the independence is easily maintained, so that the support power of the support material is easily improved.
- the weight average molecular weight of the polyalkylene glycol containing an oxybutylene group is preferably 300 to 3,000, more preferably 800 to 2,000.
- the weight average molecular weight of the polyalkylene glycol containing an oxybutylene group is at least the above lower limit value, it is easy to suppress the bleeding of the support material when the support material composition is cured.
- the bleeding is a phenomenon in which a liquid component seeps out from the inside of the cured support material to the surface of the support material.
- the weight average molecular weight of the polyalkylene glycol containing an oxybutylene group is not more than the above upper limit value, it is easy to improve the discharge stability of the support material composition.
- the polyalkylene glycol containing an oxybutylene group may be used alone or in combination of two or more.
- the content of the polyalkylene glycol containing an oxybutylene group having a weight average molecular weight within the above range is preferably a polyalkylene glycol containing an oxybutylene group. It is 80% by mass or more, more preferably 90% by mass or more, still more preferably 95% by mass or more, and particularly preferably 100% by mass, based on the total amount of glycol.
- the support material composition contained in the material jet stereolithography composition set of the present invention preferably contains a water-soluble monofunctional ethylenically unsaturated monomer in addition to the polyalkylene glycol containing an oxybutylene group.
- the water-soluble monofunctional ethylenically unsaturated monomer is polymerized to become a constituent component of the support material and exert a supporting power.
- the water-soluble monofunctional ethylenically unsaturated monomer is water-soluble, it tends to impart hardness to the support material and improve the support ability.
- water-soluble monofunctional ethylenically unsaturated monomer examples include hydroxyl group-containing (meth) acrylates having 5 to 15 carbon atoms (C) [hydroxyethyl (meth) acrylate, hydroxypropyl (meth) acrylate and 4-hydroxybutyl.
- the content of the water-soluble monofunctional ethylenically unsaturated monomer is preferably 15 to 80 parts by mass, more preferably 22 to 76 parts by mass, and further preferably 25 to 73 parts by mass with respect to 100 parts by mass of the support material composition. It is a mass part.
- the content is at least the above lower limit value, the supporting force of the support material is likely to be improved, and when the content is at least the above upper limit value, the water removability of the support material is likely to be improved.
- the support material composition included in the material jet stereolithography composition set of the present invention may further contain a photopolymerization initiator.
- the photopolymerization initiator contained in the support material composition is not particularly limited, and examples thereof include photopolymerization initiators similar to those of the model material composition described above, and preferred photopolymerization initiators are also the same as those of the model material composition. ..
- the content of the photopolymerization initiator is preferably 1 to 20 parts by mass with respect to 100 parts by mass of the support material composition.
- the content of the photopolymerization initiator is within the above range, it is easy to sufficiently reduce the unreacted polymerization component and sufficiently improve the curability of the support material.
- the support material composition contained in the material jet stereolithography composition set of the present invention preferably further contains a chain transfer agent.
- the chain transfer agent is not particularly limited as long as it is a compound that functions as a chain transfer agent for a radical reaction.
- a chain transfer agent By using a chain transfer agent, the molecular weight of the cured product is reduced when the composition is irradiated with light and photocured.
- the low-molecular-weight cured support material tends to retain its solubility in water even when the model material composition is mixed. Therefore, the low-molecular-weight cured support material is less likely to remain on the surface of the photo-cured model material during the water removal treatment.
- chain transfer agent examples include thiol compounds such as 2-mercaptobenzothiazole and ⁇ -mercaptoxylpropyltrimethoxysilane, 2,4-diphenyl-4-methyl-pentene and the like.
- the content of the chain transfer agent is preferably 0.1 to 5 parts by mass, more preferably 0.2 to 4 parts by mass, and further preferably 0.3 to 3 parts by mass with respect to 100 parts by mass of the support material composition. Is the amount of.
- the content is at least the above lower limit value, it is easy to suppress a decrease in solubility in water even when the model material composition is mixed. Further, when the content is not more than the above upper limit value, the support material is likely to be cured and the support force is likely to be improved.
- the support material composition contained in the material jet stereolithography composition set of the present invention preferably further contains a water-soluble organic solvent.
- the water-soluble organic solvent has the effect of adjusting the viscosity of the support material composition so as to be suitable for discharge by the material jet stereolithography method.
- water-soluble organic solvent examples include ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, dipropylene glycol, 2-pyrrolidone, N-methyl-2-pyrrolidone, 1,2-propanediol, and 1,3-propanediol.
- the content of the water-soluble organic solvent is preferably 30 parts by mass or less, and preferably 5 parts by mass or more, based on 100 parts by mass of the support material composition.
- the content of the water-soluble organic solvent is within the above range, it is easy to improve the removability of the support material by water or a water-soluble solvent without lowering the support force of the support material.
- the support material composition may further contain additives such as a surface conditioner and a storage stabilizer in addition to the above components.
- additives such as a surface conditioner and a storage stabilizer in addition to the above components.
- examples of the surface conditioner and the storage stabilizer include compounds similar to the surface conditioner and the storage stabilizer that may be contained in the model material composition.
- the content thereof is preferably 0.005 to 3.0 parts by mass with respect to 100 parts by mass of the support material composition.
- the content is at least the above lower limit value, it is easy to adjust the surface tension of the support material composition within an appropriate range. Further, when the content is not more than the above upper limit value, the formation of undissolved substances in the support material composition is suppressed, and foaming is likely to be difficult.
- the content thereof is preferably 0.005 to 1 part by mass, more preferably 0.05 to 0, with respect to 100 parts by mass of the support material composition. 5 parts by mass.
- the viscosity of the support material composition in the present invention is preferably 1 to 500 mPa ⁇ s, more preferably 20 to 400 mPa ⁇ s at 25 ° C. from the viewpoint of improving the discharge property from the material jet nozzle. ..
- the above viscosity measurement can be performed using an R100 type viscometer in accordance with JIS Z8803.
- the method for producing the support material composition is not particularly limited, and for example, it can be produced by uniformly mixing the components constituting the support material composition using a mixing stirrer or the like.
- a stereolithography (or) by a stereolithography method for example, a material jet stereolithography method.
- a three-dimensional object can be formed.
- the method for producing a stereolithographic product from the model material composition or the stereolithography composition set of the present invention is not particularly limited.
- the model material composition is photocured to obtain a model material
- a support material composition is used. Examples thereof include a method including a step of obtaining a support material by photocuring and a step of removing the support material from the model material.
- the data of the model material composition which is laminated by the material jet method to form the three-dimensional model, and the three-dimensional model in the process of being manufactured are supported.
- Data of the support material composition to be used is prepared, slice data for ejecting each composition is further prepared by a material jet type 3D printer, and each composition of the model material composition and the support material composition is prepared based on the prepared slice data.
- the photocuring treatment may be repeated layer by layer to prepare a stereolithographic product composed of a photocured product (model material) of the model material composition and a photocured product (support material) of the support material composition.
- Examples of the light that cures the model material composition and the support material composition include active energy rays such as far infrared rays, infrared rays, visible rays, near ultraviolet rays, ultraviolet rays, electron beams, ⁇ rays, ⁇ rays and X-rays.
- active energy rays such as far infrared rays, infrared rays, visible rays, near ultraviolet rays, ultraviolet rays, electron beams, ⁇ rays, ⁇ rays and X-rays.
- near-ultraviolet rays or ultraviolet rays are preferable from the viewpoint of ease and efficiency of curing work.
- the light source examples include conventionally known high-pressure mercury lamps, metal halide lamps, UV-LEDs, and the like.
- the LED method is preferable from the viewpoint that the equipment can be miniaturized and the power consumption is low.
- the amount of light is preferably 200 to 500 mJ / cm 2 from the viewpoint of hardness and dimensional accuracy of the modeled product.
- a UV-LED When a UV-LED is used as a light source, it is preferable to use a UV-LED having a center wavelength of 385 to 415 nm because the light can easily reach deep layers and the hardness and dimensional accuracy of the modeled object can be improved.
- each layer constituting the stereolithography is preferably thin from the viewpoint of molding accuracy, but is preferably 5 to 30 ⁇ m from the viewpoint of the balance with the molding speed.
- the obtained stereolithography is a combination of a model material and a support material.
- the support material can be removed from such a stereolithographic object to obtain a stereolithographic article as a model material.
- the support material is preferably removed, for example, by immersing the modeled product obtained in a removing solvent that dissolves the support material, making the support material flexible, and then removing the support material from the surface of the model material with a brush or the like. .
- Water, a water-soluble solvent, for example, a glycol-based solvent, an alcohol-based solvent, or the like may be used as the solvent for removing the support material. These may be used alone or in combination of two or more.
- Table 1 below shows the abbreviations and details of the raw materials used in the examples and comparative examples.
- the glass transition temperature Tg of monomer A in Table 1 was measured according to the following method. [Preparation of homopolymer of monomer A and measurement of glass transition temperature] A 5% by mass photopolymerization initiator (D) was mixed with the monomer A to prepare a composition for measuring the glass transition temperature (Tg) of the monomer A. The Tg measurement composition was dropped onto the aluminum container for measurement, and then the Tg measurement composition was cured by irradiating the Tg measurement composition with ultraviolet rays having an integrated light intensity of 500 mJ / cm 2 with a metal halide lamp to prepare a measurement sample. The glass transition temperature of the obtained measurement sample was measured by a differential scanning calorimeter (DSC) under the following conditions. (Measurement condition) Measuring device: DSC8230 (manufactured by Rigaku) Temperature rise rate: 10 ° C / min Scanning temperature: 30-200 ° C
- the coefficient of linear expansion of monomer B and monomer C in Table 1 was measured according to the following method. [Preparation of homopolymers of monomer B and monomer C and measurement of coefficient of linear expansion] A photopolymerization initiator (D) of 5% by mass was mixed with each of the monomers of the monomer B and the monomer C to prepare a composition for measuring the coefficient of linear expansion of the monomer B and the monomer C, respectively. .. Spacers with a thickness of 5 mm were arranged on the four sides of the upper surface of a glass plate (trade name "GLASS PLATE", manufactured by AS ONE Corporation, 200 mm x 200 mm x thickness 5 mm) and partitioned into a rectangle of 10 mm x 5 mm.
Landscapes
- Chemical & Material Sciences (AREA)
- Engineering & Computer Science (AREA)
- Materials Engineering (AREA)
- Manufacturing & Machinery (AREA)
- Medicinal Chemistry (AREA)
- Organic Chemistry (AREA)
- Polymers & Plastics (AREA)
- Health & Medical Sciences (AREA)
- Chemical Kinetics & Catalysis (AREA)
- Physics & Mathematics (AREA)
- Mechanical Engineering (AREA)
- Optics & Photonics (AREA)
- Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
Priority Applications (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| US17/637,926 US12403647B2 (en) | 2019-09-12 | 2020-09-10 | Photo fabrication resin composition, model material composition, and photo-cured product thereof, and photo fabrication composition set |
| JP2021545589A JP7649747B2 (ja) | 2019-09-12 | 2020-09-10 | 光造形用樹脂組成物、モデル材組成物、およびその光硬化物、ならびに光造形用組成物セット |
Applications Claiming Priority (2)
| Application Number | Priority Date | Filing Date | Title |
|---|---|---|---|
| JP2019166550 | 2019-09-12 | ||
| JP2019-166550 | 2019-09-12 |
Publications (1)
| Publication Number | Publication Date |
|---|---|
| WO2021049576A1 true WO2021049576A1 (ja) | 2021-03-18 |
Family
ID=74865704
Family Applications (1)
| Application Number | Title | Priority Date | Filing Date |
|---|---|---|---|
| PCT/JP2020/034322 Ceased WO2021049576A1 (ja) | 2019-09-12 | 2020-09-10 | 光造形用樹脂組成物、モデル材組成物、およびその光硬化物、ならびに光造形用組成物セット |
Country Status (3)
| Country | Link |
|---|---|
| US (1) | US12403647B2 (cg-RX-API-DMAC7.html) |
| JP (1) | JP7649747B2 (cg-RX-API-DMAC7.html) |
| WO (1) | WO2021049576A1 (cg-RX-API-DMAC7.html) |
Cited By (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| WO2025225711A1 (ja) * | 2024-04-26 | 2025-10-30 | マクセル株式会社 | 水検知装置、水検知システム、水検知装置用樹脂組成物及び水検知装置の製造方法 |
| EP4541560A4 (en) * | 2022-06-20 | 2026-06-03 | Zeon Corp | RESIN MIX FOR 3D PRINTER MANUFACTURING, 3D PRINTER MANUFACTURING MATERIAL, MANUFACTURED BODY AND MANUFACTURING PROCESS |
Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2004059601A (ja) * | 2002-07-24 | 2004-02-26 | Mitsubishi Rayon Co Ltd | 光学的立体造形用樹脂組成物、及び立体造形物 |
| JP2016160372A (ja) * | 2015-03-03 | 2016-09-05 | 東洋インキScホールディングス株式会社 | 光学的立体造形用活性エネルギー線重合性樹脂組成物、及び立体造形物 |
| JP2017165804A (ja) * | 2016-03-14 | 2017-09-21 | 日立マクセル株式会社 | モデル材用樹脂組成物、および、光造形品の製造方法 |
| WO2019102695A1 (ja) * | 2017-11-22 | 2019-05-31 | マクセルホールディングス株式会社 | モデル材用組成物 |
| JP2020083949A (ja) * | 2018-11-19 | 2020-06-04 | キヤノン株式会社 | 光硬化性材料組成物およびその硬化物 |
Family Cites Families (3)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP4222120B2 (ja) | 2002-10-07 | 2009-02-12 | Jsr株式会社 | 光導波路形成用感光性樹脂組成物および光導波路 |
| JP6586284B2 (ja) | 2014-06-20 | 2019-10-02 | 株式会社キーエンス | インクジェット光造形法における光造形品形成用モデル材及び光造形品の製造方法 |
| WO2017025380A1 (en) * | 2015-08-07 | 2017-02-16 | Arkema France | One-part curable soft feel coatings |
-
2020
- 2020-09-10 JP JP2021545589A patent/JP7649747B2/ja active Active
- 2020-09-10 US US17/637,926 patent/US12403647B2/en active Active
- 2020-09-10 WO PCT/JP2020/034322 patent/WO2021049576A1/ja not_active Ceased
Patent Citations (5)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| JP2004059601A (ja) * | 2002-07-24 | 2004-02-26 | Mitsubishi Rayon Co Ltd | 光学的立体造形用樹脂組成物、及び立体造形物 |
| JP2016160372A (ja) * | 2015-03-03 | 2016-09-05 | 東洋インキScホールディングス株式会社 | 光学的立体造形用活性エネルギー線重合性樹脂組成物、及び立体造形物 |
| JP2017165804A (ja) * | 2016-03-14 | 2017-09-21 | 日立マクセル株式会社 | モデル材用樹脂組成物、および、光造形品の製造方法 |
| WO2019102695A1 (ja) * | 2017-11-22 | 2019-05-31 | マクセルホールディングス株式会社 | モデル材用組成物 |
| JP2020083949A (ja) * | 2018-11-19 | 2020-06-04 | キヤノン株式会社 | 光硬化性材料組成物およびその硬化物 |
Cited By (2)
| Publication number | Priority date | Publication date | Assignee | Title |
|---|---|---|---|---|
| EP4541560A4 (en) * | 2022-06-20 | 2026-06-03 | Zeon Corp | RESIN MIX FOR 3D PRINTER MANUFACTURING, 3D PRINTER MANUFACTURING MATERIAL, MANUFACTURED BODY AND MANUFACTURING PROCESS |
| WO2025225711A1 (ja) * | 2024-04-26 | 2025-10-30 | マクセル株式会社 | 水検知装置、水検知システム、水検知装置用樹脂組成物及び水検知装置の製造方法 |
Also Published As
| Publication number | Publication date |
|---|---|
| JP7649747B2 (ja) | 2025-03-21 |
| US12403647B2 (en) | 2025-09-02 |
| US20220281157A1 (en) | 2022-09-08 |
| JPWO2021049576A1 (cg-RX-API-DMAC7.html) | 2021-03-18 |
Similar Documents
| Publication | Publication Date | Title |
|---|---|---|
| JP6571297B2 (ja) | 光造形用インクセット、光造形品、及び、光造形品の製造方法 | |
| TWI685415B (zh) | 模型材用組成物 | |
| JP6405397B2 (ja) | エネルギー線硬化型インクジェットインク組成物 | |
| JP7068270B2 (ja) | モデル材インクセット、サポート材組成物、インクセット、立体造形物および立体造形物の製造方法 | |
| JP7649747B2 (ja) | 光造形用樹脂組成物、モデル材組成物、およびその光硬化物、ならびに光造形用組成物セット | |
| JP7186508B2 (ja) | モデル材用組成物 | |
| JP7735252B2 (ja) | モデル材クリア組成物、モデル材組成物セットおよび光造形用組成物セット | |
| JP6941655B2 (ja) | モデル材用組成物 | |
| JP6941654B2 (ja) | モデル材用組成物 | |
| JP7079630B2 (ja) | モデル材用クリア組成物、光造形用組成物セットおよびその製造方法 | |
| JP7772533B2 (ja) | モデル材クリア組成物および光造形用組成物セット | |
| WO2019150644A1 (ja) | 光硬化型インクジェット記録用インク組成物およびインクセット | |
| JP2024145914A (ja) | インクジェットインク組成物およびその製造方法 | |
| JP7217160B2 (ja) | モデル材クリア組成物 | |
| JP2021130200A (ja) | 光造形用組成物セット、光造形品、及び光造形品の製造方法 | |
| JP2024176935A (ja) | モデル材用組成物、造形物、およびインクジェット光造形用組成物セット | |
| WO2019230135A1 (ja) | 光造形用インクセット、及び、光造形品の製造方法 | |
| JP2021130201A (ja) | 光造形用組成物セット |
Legal Events
| Date | Code | Title | Description |
|---|---|---|---|
| 121 | Ep: the epo has been informed by wipo that ep was designated in this application |
Ref document number: 20863905 Country of ref document: EP Kind code of ref document: A1 |
|
| ENP | Entry into the national phase |
Ref document number: 2021545589 Country of ref document: JP Kind code of ref document: A |
|
| NENP | Non-entry into the national phase |
Ref country code: DE |
|
| 122 | Ep: pct application non-entry in european phase |
Ref document number: 20863905 Country of ref document: EP Kind code of ref document: A1 |
|
| WWG | Wipo information: grant in national office |
Ref document number: 17637926 Country of ref document: US |