WO2020003857A1 - Film de polarisation protégé d'un seul côté avec une couche adhésive, dispositif d'affichage d'image et procédé de production continu associé - Google Patents

Film de polarisation protégé d'un seul côté avec une couche adhésive, dispositif d'affichage d'image et procédé de production continu associé Download PDF

Info

Publication number
WO2020003857A1
WO2020003857A1 PCT/JP2019/021065 JP2019021065W WO2020003857A1 WO 2020003857 A1 WO2020003857 A1 WO 2020003857A1 JP 2019021065 W JP2019021065 W JP 2019021065W WO 2020003857 A1 WO2020003857 A1 WO 2020003857A1
Authority
WO
WIPO (PCT)
Prior art keywords
adhesive layer
polarizing film
pressure
sensitive adhesive
weight
Prior art date
Application number
PCT/JP2019/021065
Other languages
English (en)
Japanese (ja)
Inventor
藤田 雅人
有 森本
卓 江原
雄祐 外山
Original Assignee
日東電工株式会社
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 日東電工株式会社 filed Critical 日東電工株式会社
Priority to KR1020217000367A priority Critical patent/KR20210023976A/ko
Priority to CN201980032036.9A priority patent/CN112119332B/zh
Publication of WO2020003857A1 publication Critical patent/WO2020003857A1/fr

Abstract

L'objectif de la présente invention est de fournir un film de polarisation protégé d'un seul côté avec une couche adhésive, le film présentant une aptitude à une remise en état initial, une durabilité et une stabilité de conduction électrique excellentes dans un environnement à température élevée et/ou à humidité élevée et ne se détachant pas facilement d'un substrat de verre, ou similaire, même lorsqu'il est exposé à un environnement dans lequel se produit la condensation de rosée. Ce film de polarisation protégé d'un seul côté avec une couche adhésive comprend : un film de polarisation protégé d'un seul côté ayant un film protecteur sur une seule surface d'un polariseur ; et une couche adhésive, directement ou par l'intermédiaire d'une couche de revêtement, sur le côté polariseur du film de polarisation protégé sur un seul côté. La couche adhésive contient un polymère (méth)acrylique en tant que polymère de base, a un taux de changement de poids de 1,1 % ou plus, une force adhésive P0 de 10 N/25 mm ou moins avant immersion dans l'eau, et une force adhésive P1 de 1,6 N/25 mm ou plus après immersion pendant deux heures dans l'eau.
PCT/JP2019/021065 2018-06-26 2019-05-28 Film de polarisation protégé d'un seul côté avec une couche adhésive, dispositif d'affichage d'image et procédé de production continu associé WO2020003857A1 (fr)

Priority Applications (2)

Application Number Priority Date Filing Date Title
KR1020217000367A KR20210023976A (ko) 2018-06-26 2019-05-28 점착제층을 구비한 편보호 편광 필름, 화상 표시 장치 및 그 연속 제조 방법
CN201980032036.9A CN112119332B (zh) 2018-06-26 2019-05-28 带粘合剂层的单侧保护偏振膜、图像显示装置及其连续制造方法

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2018-121207 2018-06-26
JP2018121207A JP7142497B2 (ja) 2018-06-26 2018-06-26 粘着剤層付片保護偏光フィルム、画像表示装置およびその連続製造方法

Publications (1)

Publication Number Publication Date
WO2020003857A1 true WO2020003857A1 (fr) 2020-01-02

Family

ID=68986415

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2019/021065 WO2020003857A1 (fr) 2018-06-26 2019-05-28 Film de polarisation protégé d'un seul côté avec une couche adhésive, dispositif d'affichage d'image et procédé de production continu associé

Country Status (5)

Country Link
JP (1) JP7142497B2 (fr)
KR (1) KR20210023976A (fr)
CN (1) CN112119332B (fr)
TW (1) TWI812726B (fr)
WO (1) WO2020003857A1 (fr)

Families Citing this family (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP7291475B2 (ja) * 2018-12-04 2023-06-15 三星エスディアイ株式会社 光学フィルム用粘着剤、粘着剤層、光学部材、および画像表示装置
JP2022027097A (ja) * 2020-07-31 2022-02-10 日東電工株式会社 粘着剤層付き偏光フィルム、画像表示パネル、画像表示パネルの製造方法及び粘着剤層

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2007211091A (ja) * 2006-02-08 2007-08-23 Nitto Denko Corp 粘着剤組成物、粘着剤層、および粘着剤付光学部材
US20100091223A1 (en) * 2007-01-31 2010-04-15 Lg Chem, Ltd. Polarizing plate having pressure sensitive adhesive layer with improved light leakage property
JP2014132092A (ja) * 2014-04-03 2014-07-17 Nitto Denko Corp 活性エネルギー線硬化型接着剤組成物、偏光フィルムおよびその製造方法、光学フィルムおよび画像表示装置
WO2016052531A1 (fr) * 2014-09-30 2016-04-07 日東電工株式会社 Film polarisant protégé sur un côté, film polarisant pourvu d'une couche adhésive, dispositif d'affichage d'image et son procédé de fabrication continue
WO2016052549A1 (fr) * 2014-09-30 2016-04-07 日東電工株式会社 Film polarisant protégé d'un seul côté, film polarisant doté d'une couche adhésive, dispositif d'affichage d'image, et leur procédé de production en continu
WO2017094474A1 (fr) * 2015-12-01 2017-06-08 住友化学株式会社 Composition adhésive, feuille adhésive et film optique doté d'un adhésif

Family Cites Families (14)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP4991170B2 (ja) * 2005-03-17 2012-08-01 富士フイルム株式会社 光学樹脂フィルム、偏光板及び液晶表示装置
JP5082480B2 (ja) 2007-02-13 2012-11-28 住友化学株式会社 薄型偏光板及びそれを用いた画像表示装置
JP2009001673A (ja) 2007-06-21 2009-01-08 Nitto Denko Corp 水分散型粘着剤組成物および粘着フィルム
JP5250292B2 (ja) 2007-05-02 2013-07-31 日東電工株式会社 粘着型光学フィルム
JP5379410B2 (ja) 2008-03-14 2013-12-25 日東電工株式会社 光学フィルム用粘着剤組成物、粘着型光学フィルムおよび画像表示装置
JP2010044211A (ja) 2008-08-12 2010-02-25 Sumitomo Chemical Co Ltd 偏光板及びそれを用いた画像表示装置
JP5300776B2 (ja) * 2010-03-31 2013-09-25 富士フイルム株式会社 偏光フィルム、表示装置、及びその製造方法
JP4691205B1 (ja) 2010-09-03 2011-06-01 日東電工株式会社 薄型高機能偏光膜を含む光学フィルム積層体の製造方法
JP2012247574A (ja) 2011-05-26 2012-12-13 Nitto Denko Corp 粘着型偏光板および画像表示装置
JP5930636B2 (ja) 2011-09-27 2016-06-08 住友化学株式会社 偏光板
JP6423574B2 (ja) 2012-08-31 2018-11-14 日東電工株式会社 粘着剤層付偏光フィルムおよび画像表示装置
KR101914815B1 (ko) * 2013-09-30 2018-11-05 주식회사 엘지화학 광학 필름용 수지 조성물, 이를 이용하여 형성된 광학 필름, 이를 포함하는 편광판 및 화상 표시 장치
JP6106205B2 (ja) 2014-03-31 2017-03-29 日東電工株式会社 光学フィルム用粘着剤組成物、光学フィルム用粘着剤層、粘着剤層付光学フィルムおよび画像表示装置
JP6077618B2 (ja) 2014-09-30 2017-02-08 日東電工株式会社 片保護偏光フィルム、粘着剤層付偏光フィルム、画像表示装置およびその連続製造方法

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2007211091A (ja) * 2006-02-08 2007-08-23 Nitto Denko Corp 粘着剤組成物、粘着剤層、および粘着剤付光学部材
US20100091223A1 (en) * 2007-01-31 2010-04-15 Lg Chem, Ltd. Polarizing plate having pressure sensitive adhesive layer with improved light leakage property
JP2014132092A (ja) * 2014-04-03 2014-07-17 Nitto Denko Corp 活性エネルギー線硬化型接着剤組成物、偏光フィルムおよびその製造方法、光学フィルムおよび画像表示装置
WO2016052531A1 (fr) * 2014-09-30 2016-04-07 日東電工株式会社 Film polarisant protégé sur un côté, film polarisant pourvu d'une couche adhésive, dispositif d'affichage d'image et son procédé de fabrication continue
WO2016052549A1 (fr) * 2014-09-30 2016-04-07 日東電工株式会社 Film polarisant protégé d'un seul côté, film polarisant doté d'une couche adhésive, dispositif d'affichage d'image, et leur procédé de production en continu
WO2017094474A1 (fr) * 2015-12-01 2017-06-08 住友化学株式会社 Composition adhésive, feuille adhésive et film optique doté d'un adhésif

Also Published As

Publication number Publication date
CN112119332B (zh) 2022-11-08
CN112119332A (zh) 2020-12-22
TWI812726B (zh) 2023-08-21
JP2020003576A (ja) 2020-01-09
TW202000823A (zh) 2020-01-01
KR20210023976A (ko) 2021-03-04
JP7142497B2 (ja) 2022-09-27

Similar Documents

Publication Publication Date Title
US9134460B2 (en) Adhesive composition, adhesive layer, polarizing film provided with adhesive layer, and image formation device
JP6125063B2 (ja) 粘着剤層付偏光フィルム、その製造方法並びに画像表示装置およびその連続製造方法
KR20140094502A (ko) 점착제 조성물, 점착제층, 점착제층 형성 편광 필름 및 화상 형성 장치
JP2020177243A (ja) 粘着剤層付片保護偏光フィルム、画像表示装置およびその連続製造方法
WO2017122732A1 (fr) Film polarisant protégé sur un côté à couche adhésive, dispositif d'affichage d'image, et procédé de production en continu associé
JP6763102B2 (ja) 粘着剤層付片保護偏光フィルム、画像表示装置およびその連続製造方法
JP7153459B2 (ja) 粘着剤層、粘着剤層付片保護偏光フィルム、画像表示装置およびその連続製造方法
WO2020003857A1 (fr) Film de polarisation protégé d'un seul côté avec une couche adhésive, dispositif d'affichage d'image et procédé de production continu associé
WO2018181715A1 (fr) Couche adhésive autocollante, film polarisant protégé sur un côté comportant une couche adhésive autocollante, dispositif d'affichage d'image, et procédé de production continue associé
WO2018181014A1 (fr) Film polarisant protege par un seul côté avec couche adhésive sensible à la pression, dispositif d'affichage d'image et procédé de production continu à cet effet
WO2016129632A1 (fr) Film de polarisation pourvu d'une couche adhésive, procédé de fabrication de celui-ci, et dispositif d'affichage d'image et procédé de fabrication de celui-ci
WO2018180999A1 (fr) Film polarisant protege par un seul côté avec couche adhésive sensible à la pression, dispositif d'affichage d'image et procédé de production continu à cet effet
JP7190268B2 (ja) 粘着剤層付偏光フィルム及びその剥離方法、並びに画像表示装置
KR102460885B1 (ko) 점착제층, 점착제층을 구비한 편보호 편광 필름, 화상 표시 장치 및 그 연속 제조 방법

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 19826680

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 20217000367

Country of ref document: KR

Kind code of ref document: A

122 Ep: pct application non-entry in european phase

Ref document number: 19826680

Country of ref document: EP

Kind code of ref document: A1