WO2019011793A1 - PROCESS FOR PRODUCING SUPERABSORBENT POLYMER PARTICLES - Google Patents

PROCESS FOR PRODUCING SUPERABSORBENT POLYMER PARTICLES Download PDF

Info

Publication number
WO2019011793A1
WO2019011793A1 PCT/EP2018/068326 EP2018068326W WO2019011793A1 WO 2019011793 A1 WO2019011793 A1 WO 2019011793A1 EP 2018068326 W EP2018068326 W EP 2018068326W WO 2019011793 A1 WO2019011793 A1 WO 2019011793A1
Authority
WO
WIPO (PCT)
Prior art keywords
roll crusher
fraction
polymer particles
μιη
sieve
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/EP2018/068326
Other languages
English (en)
French (fr)
Inventor
Ruediger Funk
Thomas Pfeiffer
Matthias Weismantel
Monte Peterson
Karl Possemiers
Ronny De Kaey
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
BASF SE
Original Assignee
BASF SE
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by BASF SE filed Critical BASF SE
Priority to CN201880044601.9A priority Critical patent/CN110832011B/zh
Priority to JP2020501118A priority patent/JP7229987B2/ja
Priority to KR1020207000175A priority patent/KR102563402B1/ko
Priority to US16/628,689 priority patent/US11680142B2/en
Priority to EP18734837.0A priority patent/EP3652237B1/en
Publication of WO2019011793A1 publication Critical patent/WO2019011793A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/24—Crosslinking, e.g. vulcanising, of macromolecules
    • C08J3/245—Differential crosslinking of one polymer with one crosslinking type, e.g. surface crosslinking
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B02—CRUSHING, PULVERISING, OR DISINTEGRATING; PREPARATORY TREATMENT OF GRAIN FOR MILLING
    • B02C—CRUSHING, PULVERISING, OR DISINTEGRATING IN GENERAL; MILLING GRAIN
    • B02C23/00—Auxiliary methods or auxiliary devices or accessories specially adapted for crushing or disintegrating not provided for in preceding groups or not specially adapted to apparatus covered by a single preceding group
    • B02C23/08—Separating or sorting of material, associated with crushing or disintegrating
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B02—CRUSHING, PULVERISING, OR DISINTEGRATING; PREPARATORY TREATMENT OF GRAIN FOR MILLING
    • B02C—CRUSHING, PULVERISING, OR DISINTEGRATING IN GENERAL; MILLING GRAIN
    • B02C4/00—Crushing or disintegrating by roller mills
    • B02C4/02—Crushing or disintegrating by roller mills with two or more rollers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B02—CRUSHING, PULVERISING, OR DISINTEGRATING; PREPARATORY TREATMENT OF GRAIN FOR MILLING
    • B02C—CRUSHING, PULVERISING, OR DISINTEGRATING IN GENERAL; MILLING GRAIN
    • B02C4/00—Crushing or disintegrating by roller mills
    • B02C4/28—Details
    • B02C4/30—Shape or construction of rollers
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B07—SEPARATING SOLIDS FROM SOLIDS; SORTING
    • B07B—SEPARATING SOLIDS FROM SOLIDS BY SIEVING, SCREENING, SIFTING OR BY USING GAS CURRENTS; SEPARATING BY OTHER DRY METHODS APPLICABLE TO BULK MATERIAL, e.g. LOOSE ARTICLES FIT TO BE HANDLED LIKE BULK MATERIAL
    • B07B1/00—Sieving, screening, sifting, or sorting solid materials using networks, gratings, grids, or the like
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B07—SEPARATING SOLIDS FROM SOLIDS; SORTING
    • B07B—SEPARATING SOLIDS FROM SOLIDS BY SIEVING, SCREENING, SIFTING OR BY USING GAS CURRENTS; SEPARATING BY OTHER DRY METHODS APPLICABLE TO BULK MATERIAL, e.g. LOOSE ARTICLES FIT TO BE HANDLED LIKE BULK MATERIAL
    • B07B1/00—Sieving, screening, sifting, or sorting solid materials using networks, gratings, grids, or the like
    • B07B1/46—Constructional details of screens in general; Cleaning or heating of screens
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/02—Making solutions, dispersions, lattices or gels by other methods than by solution, emulsion or suspension polymerisation techniques
    • C08J3/03—Making solutions, dispersions, lattices or gels by other methods than by solution, emulsion or suspension polymerisation techniques in aqueous media
    • C08J3/075—Macromolecular gels
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/12—Powdering or granulating
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2300/00—Characterised by the use of unspecified polymers
    • C08J2300/12—Polymers characterised by physical features, e.g. anisotropy, viscosity or electrical conductivity
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2300/00—Characterised by the use of unspecified polymers
    • C08J2300/14—Water soluble or water swellable polymers, e.g. aqueous gels
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2333/00—Characterised by the use of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Derivatives of such polymers
    • C08J2333/04—Characterised by the use of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Derivatives of such polymers esters
    • C08J2333/06—Characterised by the use of homopolymers or copolymers of compounds having one or more unsaturated aliphatic radicals, each having only one carbon-to-carbon double bond, and only one being terminated by only one carboxyl radical, or of salts, anhydrides, esters, amides, imides, or nitriles thereof; Derivatives of such polymers esters of esters containing only carbon, hydrogen, and oxygen, the oxygen atom being present only as part of the carboxyl radical
    • C08J2333/08—Homopolymers or copolymers of acrylic acid esters
    • Y—GENERAL TAGGING OF NEW TECHNOLOGICAL DEVELOPMENTS; GENERAL TAGGING OF CROSS-SECTIONAL TECHNOLOGIES SPANNING OVER SEVERAL SECTIONS OF THE IPC; TECHNICAL SUBJECTS COVERED BY FORMER USPC CROSS-REFERENCE ART COLLECTIONS [XRACs] AND DIGESTS
    • Y02—TECHNOLOGIES OR APPLICATIONS FOR MITIGATION OR ADAPTATION AGAINST CLIMATE CHANGE
    • Y02W—CLIMATE CHANGE MITIGATION TECHNOLOGIES RELATED TO WASTEWATER TREATMENT OR WASTE MANAGEMENT
    • Y02W30/00—Technologies for solid waste management
    • Y02W30/50—Reuse, recycling or recovery technologies
    • Y02W30/62—Plastics recycling; Rubber recycling

Definitions

  • the invention relates to a process for producing superabsorbent polymer particles, comprising surface postcrosslinking, classifying the surface postcrosslinked superabsorbent polymer particles, deagglomerating the separated oversize fraction using a roll crusher and recycling the deagglomerated oversize fraction before or into the classification of the surface postcrosslinked superabsorbent polymer particles.
  • Superabsorbent polymer particles are used to produce diapers, tampons, sanitary napkins and other hygiene articles, but also as water-retaining agents.
  • the superabsorbent polymer particles are often also referred to as "absorbent resins", “superabsorbents”, “ water- absorbent polymers”, “absorbent polymers”, “absorbent gelling materials”, “hydrophilic polymers” or “hydrogels”.
  • US 2004/0242761 Al teaches the deagglomeration of agglomerates that are formed during surface postcrosslinking and WO 2008/037673 Al discloses a process for separation of such agglomerates.
  • the object was achieved by a process for producing superabsorbent polymer particles, comprising polymerization of a monomer solution or suspension, comprising a) at least one ethylenically unsaturated monomer which bears acid groups and may be at least partly neutralized,
  • Roll crushers can consist of single or multiple rolls. The surface of the rolls is smooth, corrugated, or toothed. Roll crushers are described in "Perry's Chemical Engineer's
  • double toothed roll crushers are used.
  • the teeth of the double toothed roll crusher have rounded edges so that the roll crusher deagglomerates the agglomerates mainly by compression.
  • the rolls of the roll crusher have a smooth surface.
  • the surface of the rolls of the roll crusher has a roughness R z of preferably less than 25 ⁇ , more preferably of less than 15 ⁇ , most preferably of less than 5 ⁇ .
  • the roughness R z is the greatest height of the profile and is described in DIN EN ISO 4287.
  • the gap width of the roll crusher is preferably from 0.8 to 10 mm, more preferably from 0.9 to 5 mm, most preferably from 1.0 to 2 mm, wherein the gap width of the roll crusher is the smallest distance between the two surfaces that form the gap of the roll crusher.
  • the sieve for separating the oversize fraction and the midsize fraction has a mesh size from preferably 600 to 1.200 ⁇ , more preferably 700 to 1,100 ⁇ , most preferably 800 to 1,000 ⁇ .
  • the sieve for separating the undersize fraction and the midsize fraction has a mesh size from preferably 100 to 300 ⁇ , more preferably 120 to 250 ⁇ , most preferably 150 to 200 ⁇ .
  • the gap width of the roll crusher is larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the gap width of the roll crusher is preferably from 50 to 800 ⁇ , more preferably from 100 to 600 ⁇ , most preferably from 150 to 400 ⁇ , larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 600 to 1.200 ⁇ and the gap width of the roll crusher is from 50 to 800 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 600 to 1.200 ⁇ and the gap width of the roll crusher is from 100 to 600 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, more preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 600 to 1.200 ⁇ and the gap width of the roll crusher is from 150 to 400 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 700 to 1.100 ⁇ and the gap width of the roll crusher is from 50 to 800 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 700 to 1.100 ⁇ and the gap width of the roll crusher is from 100 to 600 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, more preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 700 to 1.100 ⁇ and the gap width of the roll crusher is from 150 to 400 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 800 to 1.000 ⁇ and the gap width of the roll crusher is from 50 to 800 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 800 to 1.000 ⁇ and the gap width of the roll crusher is from 100 to 600 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction, more preferably the sieve for separating the oversize fraction and the midsize fraction has a mesh size from 800 to 1.000 ⁇ and the gap width of the roll crusher is from 150 to 400 ⁇ larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the undersize fraction is recycled into the polymerization and/or the surface postcrosslinked superabsorbent polymer particles are classified using a tumbling screen machine.
  • the present invention is based on the finding that the agglomerates that are formed during the surface postcrosslinking of water-absorbent polymer particles can be easily
  • a roll crusher the agglomerates are crushed and are not milled or cut.
  • the mechanical stress during crushing can be further decreased by increasing the gap width of the roll crusher and increasing the circulation load.
  • a too high gap width results in a too high circulation load and overloading of the classification.
  • the circulation load is the rate of recycled oversize fraction based on the production rate.
  • the circulation load may be in the range from 0.02 to 0.4.
  • the present invention further provides an apparatus for sizing of surface postcrosslinked superabsorbent polymer particles, comprising a tumbling sieve machine for classifying particles into an undersize, midsize, and oversize fraction, a roll crusher for deagglomerating the oversize fraction, and a line for recycling the deagglomerated superabsorbent polymer particles before or into the tumbling sieve machine.
  • double toothed roll crushers are used.
  • the teeth of the double toothed roll crusher have rounded edges.
  • the surface of the rolls of the roll crusher has a roughness R z of preferably less than 25 ⁇ , more preferably of less than 15 ⁇ , most preferably of less than 5 ⁇ .
  • the roughness R z is the greatest height of the profile and is described in DIN EN ISO 4287.
  • the gap width of the roll crusher is preferably from 0.8 to 10 mm, more preferably from 0.9 to 5 mm, most preferably from 1.0 to 2 mm, wherein the gap width of the roll crusher is the smallest distance between the two surfaces that form the gap of the roll crusher.
  • the sieve for separating the oversize fraction and the midsize fraction has a mesh size from preferably 600 to 1.200 ⁇ , more preferably 700 to 1,100 ⁇ , most preferably 800 to 1,000 ⁇ .
  • the sieve for separating the undersize fraction and the midsize fraction has a mesh size from preferably 100 to 300 ⁇ , more preferably 120 to 250 ⁇ , most preferably 150 to 200 ⁇ .
  • the gap width of the roll crusher is larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the gap width of the roll crusher is preferably from 50 to 800 ⁇ , more preferably from 100 to 600 ⁇ , most preferably from 150 to 400 ⁇ , larger than the mesh size of the sieve for separating the oversize fraction and the midsize fraction.
  • the superabsorbent polymer particles are produced by polymerizing a monomer solution or suspension, and are typically water-insoluble.
  • the monomers a) are preferably water-soluble, i.e. the solubility in water at 23° C is typically at least 1 g/100 g of water, preferably at least 5 g/100 g of water, more preferably at least 25 g/100 g of water and most preferably at least 35 g/100 g of water.
  • Suitable monomers a) are, for example, ethylenically unsaturated carboxylic acids, such as acrylic acid, methacrylic acid and itaconic acid. Particularly preferred monomers are acrylic acid and methacrylic acid. Very particular preference is given to acrylic acid.
  • Further suitable monomers a) are, for example, ethylenically unsaturated sulfonic acids, such as styrenesulfonic acid and 2-acrylamido-2-methylpropanesulfonic acid (AMPS).
  • Impurities can have a considerable influence on the polymerization.
  • the raw materials used should therefore have a high and constant purity. It is therefore often advantageous to specially purify the monomers a). Suitable purification processes are described, for example, in WO 2002/055469 Al, WO 2003/078378 Al and WO 2004/035514 Al.
  • a suitable monomer a) is, for example, acrylic acid purified according to WO 2004/035514 Al and comprising 99.8460% by weight of acrylic acid, 0.0950% by weight of acetic acid, 0.0332% by weight of water, 0.0203% by weight of propionic acid, 0.0001% by weight of furfurals, 0.0001% by weight of maleic anhydride, 0.0003% by weight of diacrylic acid and 0.0050% by weight of hydroquinone monomethyl ether.
  • the proportion of acrylic acid and/or salts thereof in the total amount of monomers a) is preferably at least 50 mol%, more preferably at least 90 mol%, most preferably at least 95 mol%.
  • the monomers a) typically comprise polymerization inhibitors, preferably hydroquinone monoethers, as storage stabilizers.
  • the monomer solution comprises preferably up to 250 ppm by weight, preferably at most 130 ppm by weight, more preferably at most 70 ppm by weight, and preferably at least 10 ppm by weight, more preferably at least 30 ppm by weight and especially around 50 ppm by weight, of hydroquinone monoether, based in each case on the unneutralized monomer a).
  • the monomer solution can be prepared by using an ethylenically unsaturated monomer bearing acid groups with an appropriate content of hydroquinone monoether.
  • Preferred hydroquinone monoethers are hydroquinone monomethyl ether (MEHQ) and/or alpha-tocopherol (vitamin E).
  • Suitable crosslinkers b) are compounds having at least two groups suitable for crosslinking. Such groups are, for example, ethylenically unsaturated groups which can be polymerized free-radically into the polymer chain, and functional groups which can form covalent bonds with the acid groups of the monomer a).
  • polyvalent metal salts which can form coordinate bonds with at least two acid groups of the monomer a) are also suitable as crosslinkers b).
  • Crosslinkers b) are preferably compounds having at least two polymerizable groups which can be polymerized free-radically into the polymer network.
  • Suitable crosslinkers b) are, for example, ethylene glycol dimethacrylate, diethylene glycol diacrylate, polyethylene glycol diacrylate, allyl methacrylate, trimethylolpropane triacrylate, triallylamine,
  • Very particularly preferred crosslin kers b) are the polyethoxylated and/or -propoxylated glycerols which have been esterified with acrylic acid or methacrylic acid to give di- or triacrylates, as described, for exam ple, in WO 2003/104301 Al.
  • Di- and/or triacrylates of 3- to 10-tu ply ethoxylated glycerol are particu larly advantageous.
  • Very particu lar preference is given to di- or triacrylates of 1- to 5-tu ply ethoxylated and/or propoxylated glycerol.
  • Most preferred are the triacrylates of 3- to 5-tu ply ethoxylated and/or propoxylated glycerol, especially the triacrylate of 3-tu ply ethoxylated glycerol.
  • the amou nt of crosslin ker b) is preferably 0.05 to 1.5% by weight, more preferably 0.1 to 1% by weight and most preferably 0.2 to 0.6% by weight, based in each case on monomer a).
  • the centrifuge retention capacity falls and the absorption u nder a pressu re of 21.0 g/cm 2 passes through a maximum.
  • the initiators c) used may be all com pou nds which generate free radicals under the polymerization conditions, for example thermal initiators, redox initiators, photoinitiators. Suitable redox initiators are sodiu m peroxodisu lfate/ascorbic acid, hydrogen
  • the reducing component used is preferably disodium 2-hydroxy-2-su lfonatoacetate or a mixtu re of disodium 2-hydroxy-2-su lfinatoacetate, disodium 2-hydroxy-2-su lfonatoacetate and sodiu m bisu lfite.
  • mixtu res are obtainable as Bruggolite ® FF6 and Bruggolite ® FF7 (Bruggeman n Chemicals; Heilbron n; Germany).
  • Ethylenically unsatu rated monomers d) copolymerizable with the ethylenically u nsatu rated monomers a) bearing acid grou ps are, for exam ple, acrylamide, methacrylamide,
  • the water-soluble polymers e) used may be polyvinyl alcohol, polyvinylpyrrolidone, starch, starch derivatives, modified cellulose, such as methylcellulose or hydroxyethylcellulose, gelatin, polyglycols or polyacrylic acids, preferably starch, starch derivatives and modified cellulose.
  • an aqueous monomer solution is used.
  • the water content of the monomer solution is preferably from 40 to 75% by weight, more preferably from 45 to 70% by weight and most preferably from 50 to 65% by weight.
  • monomer suspensions i.e. monomer solutions with excess monomer a), for example sodium acrylate. With rising water content, the energy requirement in the subsequent drying rises, and, with falling water content, the heat of polymerization can only be removed inadequately.
  • the preferred polymerization inhibitors require dissolved oxygen.
  • the monomer solution can therefore be freed of dissolved oxygen before the polymerization by inertization, i.e. flowing an inert gas through, preferably nitrogen or carbon dioxide.
  • the oxygen content of the monomer solution is preferably lowered before the polymerization to less than 1 ppm by weight, more preferably to less than 0.5 ppm by weight, most preferably to less than 0.1 ppm by weight.
  • triphosphoric acid polyphosphoric acid, citric acid, tartaric acid, or salts thereof.
  • iminodiacetic acid hydroxyethyliminodiacetic acid, nitrilotriacetic acid, nitrilotripropionic acid, ethylenediaminetetraacetic acid,
  • diethylenetriaminepentaacetic acid triethylenetetraaminehexaacetic acid, N,N-bis(2- hydroxyethyl)glycine and trans-l,2-diaminocyclohexanetetraacetic acid, and salts thereof.
  • the amount used is typically 1 to 30000 ppm based on the monomers a), preferably 10 to 1000 ppm, preferentially 20 to 600 ppm, more preferably 50 to 400 ppm, most preferably 100 to 300 ppm.
  • the monomer solution or suspension is polymerized.
  • Suitable reactors are, for example, kneading reactors or belt reactors. In the kneader, the polymer gel formed in the
  • polymerization of an aqueous monomer solution or suspension is comminuted continuously by, for example, contrarotatory stirrer shafts, as described in WO 2001/038402 Al.
  • Polymerization on the belt is described, for example, in DE 3825366 Al and US 6,241,928.
  • Polymerization in a belt reactor forms a polymer gel which has to be comminuted in a further process step, for example in an extruder or kneader.
  • the comminuted polymer gel obtained by means of a kneader can additionally be extruded.
  • the acid groups of the resulting polymer gels have typically been partially neutralized.
  • Neutralization is preferably carried out at the monomer stage. This is typically accomplished by mixing in the neutralizing agent as an aqueous solution or preferably also as a solid.
  • the degree of neutralization is preferably from 50 to 90 mol%, more preferably from 60 to 85 mol% and most preferably from 65 to 80 mol%, for which the customary neutralizing agents can be used, preferably alkali metal hydroxides, alkali metal oxides, alkali metal carbonates or alkali metal hydrogencarbonates and also mixtures thereof.
  • alkali metal salts it is also possible to use ammonium salts.
  • Particularly preferred alkali metals are sodium and potassium, but very particular preference is given to sodium hydroxide, sodium carbonate or sodium hydrogencarbonate and also mixtures thereof.
  • the polymer gel is neutralized at least partly after the polymerization, the polymer gel is preferably comminuted mechanically, for example by means of an extruder, in which case the neutralizing agent can be sprayed, sprinkled or poured on and then carefully mixed in. To this end, the gel mass obtained can be repeatedly extruded for homogenization.
  • the resulting polymer gel is dried.
  • the driers are not subject to any restriction. However, the drying of the polymer gel is preferably performed with a belt drier until the residual moisture content is preferably 0.5 to 10% by weight, more preferably 1 to 7% by weight and most preferably 2 to 5% by weight, the residual moisture content being determined by EDANA recommended test method No. WSP 230.2-05 "Mass Loss Upon Heating". In the case of too high a residual moisture content, the dried polymer gel has too low a glass transition temperature T g and can be processed further only with difficulty.
  • the dried polymer gel is too brittle and, in the subsequent grinding steps, undesirably large amounts of polymer particles with an excessively low particle size are obtained (“fines").
  • the solids content of the gel before the drying is preferably from 25 to 90% by weight, more preferably from 35 to 70% by weight and most preferably from 40 to 60% by weight.
  • a fluidized bed drier or a paddle drier may optionally also be used for drying purposes.
  • the apparatus used for grinding may typically be single- or multistage roll mills, preferably two- or three-stage mills, pin mills, hammer mills or vibratory mills.
  • the mean particle size of the polymer particles removed as the product fraction is preferably at least 200 ⁇ , more preferably from 250 to 600 ⁇ and very particularly from 300 to 500 ⁇ .
  • the mean particle size of the product fraction may be determined by means of EDANA recommended test method No. WSP 220.2-05 "Particle Size Distribution", where the proportions by mass of the screen fractions are plotted in cumulated form and the mean particle size is determined graphically.
  • the mean particle size here is the value of the mesh size which gives rise to a cumulative 50% by weight.
  • the proportion of particles with a particle size of at least 150 ⁇ is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
  • Polymer particles with too small a particle size lower the saline flow conductivity (SFC).
  • SFC saline flow conductivity
  • the proportion of excessively small polymer particles should therefore be low.
  • Excessively small polymer particles are therefore typically removed and recycled into the process. This is preferably done before, during or immediately after the polymerization, i.e. before the drying of the polymer gel.
  • the excessively small polymer particles can be moistened with water and/or aqueous surfactant before or during the recycling. It is also possible to remove excessively small polymer particles in later process steps, for example after the surface postcrosslinking or another coating step. In this case, the excessively small polymer particles recycled are surface postcrosslinked or coated in another way, for example with fumed silica.
  • the excessively small polymer particles are preferably added during the last third of the polymerization.
  • the excessively small polymer particles When the excessively small polymer particles are added at a very late stage, for example not until an apparatus connected downstream of the polymerization reactor, for example an extruder, the excessively small polymer particles can be incorporated into the resulting polymer gel only with difficulty. Insufficiently incorporated, excessively small polymer particles are, however, detached again from the dried polymer gel during the grinding, are therefore removed again in the course of classification and increase the amount of excessively small polymer particles to be recycled.
  • the proportion of particles having a particle size of at most 850 ⁇ is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
  • the proportion of particles having a particle size of at most 600 ⁇ is preferably at least 90% by weight, more preferably at least 95% by weight, most preferably at least 98% by weight.
  • Polymer particles of excessively large particle size lower the free swell rate.
  • the proportion of excessively large polymer particles shou ld therefore likewise be small.
  • Suitable surface postcrosslin kers are com pou nds which comprise grou ps which can form covalent bonds with at least two acid grou ps of the polymer particles.
  • Suitable compounds are, for example, polyfu nctional amines, polyfu nctional amido amines, polyfunctional epoxides, as described in EP 0 083 022 A2, EP 0 543 303 Al and EP 0 937 736 A2, di- or polyfunctional alcohols, as described in DE 33 14 019 Al, DE 35 23 617 Al and EP 0 450 922 A2, or ⁇ -hyd roxyalkylamides, as described in DE 102 04 938 Al and US 6,239,230.
  • su rface postcrosslin kers are cyclic carbonates
  • Preferred surface postcrosslin kers are ethylene carbonate, ethylene glycol diglycidyl ether, reaction products of polyamides with epich lorohyd rin and mixtu res of propylene glycol and 1,4-butanediol.
  • Very particu larly preferred su rface postcrosslin kers are 2-hyd roxyethyloxazolidin-2-one, oxazolidin-2-one and 1,3-propanediol.
  • su rface postcrosslin kers which com prise additional polymerizable ethylenically u nsaturated groups, as described in DE 37 13 601 Al.
  • the amou nt of surface postcrosslinker is preferably 0.001 to 2% by weight, more preferably 0.02 to 1% by weight and most preferably 0.05 to 0.2% by weight, based in each case on the polymer particles.
  • polyvalent cations are applied to the particle su rface in addition to the surface postcrosslin kers before, du ring or after the su rface postcrosslin king.
  • the polyvalent cations usable in the process according to the invention are, for example, divalent cations such as the cations of zinc, magnesium, calcium, iron and strontium, trivalent cations such as the cations of aluminum, iron, chromium, rare earths and manganese, tetravalent cations such as the cations of titanium and zirconium.
  • Possible counterions are chloride, bromide, sulfate, hydrogensulfate, carbonate, hydrogencarbonate, nitrate, phosphate, hydrogenphosphate, dihydrogenphosphate and carboxylate, such as acetate and lactate.
  • Aluminum sulfate and aluminum lactate are preferred.
  • polyamines as polyvalent cations.
  • the amount of polyvalent cation used is, for example, 0.001 to 1.5% by weight, preferably 0.005 to 1% by weight and more preferably 0.02 to 0.8% by weight, based in each case on the polymer particles.
  • the surface postcrosslinking is typically performed in such a way that a solution of the surface postcrosslinker is sprayed onto the dried polymer particles. After the spray application, the polymer particles coated with surface postcrosslinker are dried thermally, and the surface postcrosslinking reaction can take place either before or during the drying.
  • the spray application of a solution of the surface postcrosslinker is preferably performed in mixers with moving mixing tools, such as screw mixers, disk mixers and paddle mixers.
  • horizontal mixers such as paddle mixers
  • vertical mixers very particular preference to vertical mixers.
  • the distinction between horizontal mixers and vertical mixers is made by the position of the mixing shaft, i.e. horizontal mixers have a horizontally mounted mixing shaft and vertical mixers a vertically mounted mixing shaft.
  • Suitable mixers are, for example, horizontal Pflugschar ® plowshare mixers (Gebr. Lodige Maschinenbau GmbH; Paderborn; Germany), Vrieco-Nauta continuous mixers (Hosokawa Micron BV;
  • the surface postcrosslinkers are typically used in the form of an aqueous solution.
  • the penetration depth of the surface postcrosslinker into the polymer particles can be adjusted via the content of nonaqueous solvent and total amount of solvent.
  • a surfactant is advantageously added. This improves the wetting behavior and reduces the tendency to form lumps.
  • solvent mixtures for example isopropanol/water, 1,3- propanediol/water and propylene glycol/water, where the mixing ratio in terms of mass is preferably from 20:80 to 40:60.
  • the surface postcrosslinking is preferably performed in contact driers, more preferably paddle driers, most preferably disk driers.
  • Suitable driers are, for example, Hosokawa Bepex ® Horizontal Paddle Dryer (Hosokawa Micron GmbH; Leingart; Germany), Hosokawa Bepex ® Disc Dryer (Hosokawa Micron GmbH; Leingart; Germany) and Nara Paddle Dryer (NARA Machinery Europe; Frechen; Germany).
  • fluidized bed driers may also be used.
  • the surface postcrosslinking can be effected in the mixer itself, by heating the jacket or blowing in warm air.
  • a downstream drier for example a shelf drier, a rotary tube oven or a heatable screw. It is particularly advantageous to effect mixing and drying in a fluidized bed drier.
  • Preferred surface postcrosslinking temperatures are in the range of 100 to 250° C, preferably 110 to 220° C, more preferably 120 to 210° C and most preferably 130 to 200° C.
  • the preferred residence time at this temperature in the reaction mixer or drier is preferably at least 10 minutes, more preferably at least 20 minutes, most preferably at least 30 minutes, and typically at most 60 minutes.
  • the surface postcrosslinked polymer particles are classified again, excessively small and/or excessively large polymer particles being removed and recycled into the process.
  • the surface postcrosslinked polymer particles can be coated or remoisturized.
  • the remoisturizing is preferably performed at 30 to 80° C, more preferably at 35 to 70° C, most preferably at 40 to 60° C. At excessively low temperatures, the superabsorbent polymer particles tend to form lumps, and, at higher temperatures, water already evaporates to a noticeable degree.
  • the amount of water used for remoisturizing is preferably from 1 to 10% by weight, more preferably from 2 to 8% by weight and most preferably from 3 to 5% by weight. The remoisturizing increases the mechanical stability of the polymer particles and reduces their tendency to static charging.
  • Suitable coatings for improving the free swell rate and the saline flow conductivity (SFC) are, for example, inorganic inert substances, such as water-insoluble metal salts, organic polymers, cationic polymers and di- or polyvalent metal cations.
  • Suitable coatings for dust binding are, for example, polyols.
  • Suitable coatings for counteracting the undesired caking tendency of the polymer particles are, for example, fumed silica, such as Aerosil ® 200, and surfactants, such as Span ® 20.
  • the superabsorbent polymer particles produced by the process according to the invention have a centrifuge retention capacity (CRC) of typically at least 15 g/g, preferably at least 20 g/g, more preferably at least 22 g/g, especially preferably at least 24 g/g and most preferably at least 26 g/g.
  • the centrifuge retention capacity (CRC) of the superabsorbent polymer particles is typically less than 60 g/g.
  • the centrifuge retention capacity (CRC) is determined by EDANA recommended test method No. NWSP 241.0.R2 (15)" Determination of the Fluid Retention Capacity in Saline Solution by Gravimetric Measurement Following Centrifugation".
  • the superabsorbent polymer particles produced by the process according to the invention have an absorption under high load (AUHL) of typically at least 15 g/g, preferably at least 20 g/g, more preferably at least 22 g/g, especially preferably at least 24 g/g and most preferably at least 26 g/g.
  • AUHL absorption under high load
  • the absorption under high load (AUHL) of the superabsorbent polymer particles is typically less than 35 g/g.
  • the absorption under high load (AUHL) is determined by EDANA recommended test method No. WSP NWSP 242.0.R2" Gravimetric Determination of Absorption against Pressure" and a pressure of 49.2 g/cm 2 .
  • the measurements should, unless stated otherwise, be carried out at an ambient tempera ⁇ ture of 23 ⁇ 2° C and a relative atmospheric humidity of 50 ⁇ 10%.
  • the water-absorbent polymers are mixed thoroughly before the measurement.
  • centrifuge retention capacity of the water-absorbent polymer particles is determined by the EDANA recommended test method No. NWSP 241.0.R2 (15)" Determination of the Fluid Retention Capacity in Saline Solution by Gravimetric Measurement Following Centrifuga ⁇ tion", wherein for higher values of the centrifuge retention capacity lager tea bags have to be used.
  • the absorbency under high load of the water-absorbent polymer particles is determined by the EDANA recommended test method No. WSP NWSP 242.0.R2" Gravimetric Determina ⁇ tion of Absorption against Pressure" and a pressure of 49.2 g/cm 2 .
  • the saline flow conductivity is, as described in EP 0640330 Al, determined as the gel layer permeability of a swollen gel layer of water-absorbent polymer particles, although the appa ⁇ ratus described on page 19 and in figure 8 in the aforementioned patent application was modified to the effect that the glass frit (40) is no longer used, the plunger (39) consists of the same polymer material as the cylinder (37) and now comprises 21 bores having a diam- eter of 9.65mm each distributed uniformly over the entire contact surface. The procedure and the evaluation of the measurement remains unchanged from EP 0640330 Al. The flow rate is recorded automatically.
  • SFC saline flow conductivity
  • an acrylic acid/sodium acrylate solution was prepared, such that the degree of neutralization corresponds to 71 mol%.
  • the solids content of the monomer solution was 41.5% by weight.
  • crosslinker 3-tuply ethoxylated glycerol triacrylate was used as crosslinker.
  • the amount of crosslinker was 1.06 kg per t of monomer solution.
  • the free-radical polymerization was initiated by adding 1.3 kg of a 0.25% by weight aqueous hydrogen peroxide solution, 1.54 kg of a 27% by weight aqueous sodium peroxodisulfate so ⁇ lution, and 1.4 kg of a 1% by weight aqueous ascorbic acid solution, each based per t of monomer solution.
  • the throughput of the monomer solution was 18 t/h.
  • the monomer solution had a tempera ⁇ ture of 30° C at the feed.
  • the individual components were metered in the following amounts continuously into a con ⁇ tinuous kneader reactor with a capacity of 6.3 m 3 (LIST AG, Arisdorf, Switzerland):
  • the monomer solution was inertized with nitrogen.
  • the dried polymer gel was ground and screened off to a particle size fraction of 150 to 850 ⁇ .
  • the resulting base polymer exhibited a centrifuge retention capacity (CRC) of 38,7g/g, an absorbency under high load (AULOJpsi) of 7,3 g/g and a PSD of >850 ⁇ 2.5wt.%
  • the resulting base polymer was surface postcrosslinked:
  • the base pol ⁇ ymer was coated with a surface postcrosslinker solution and then dried in a NARA ® paddle dryer (GMF Gouda, Waddinxveen, the Netherlands) at 185° C for 45 minutes.
  • the paddle dryer was heated with steam having a pressure of 24bar (220° C).
  • the surface postcrosslinker solution comprised of 1.59% by weight of 2-hydroxyethyl-2 oxa- zolidone, 1.59% by weight of propandiole-1.3, 13.25% by weight of propandiole-1.2, 0.08% by weight of Sorbitanmonolaurat (Span ® 20), 11.13% by weight of aluminum tri lactate, 51.95% by weight of deionized water, and 20.41% by weight of isopropanol.
  • the surface postcrosslinked base polymer was cooled to approx.60° C in a NARA ® paddle cooler (GMF Gouda, Waddinxveen, the Netherlands). After the cooling, the superabsorbent polymer particles were again screened off to from 150 to 850 ⁇ (SXL polymer).
  • the SXL polymer was analysed and exhibited a centrifuge retention capacity (CRC) of 30.1 g/g, an absorbency under high load (AUHL) of 23.4 g/g, and a saline flow conductivity (SFC) of 52 x 10 "7 cm 3 s/g.
  • CRC centrifuge retention capacity
  • AUHL absorbency under high load
  • SFC saline flow conductivity
  • the oversize fraction (SXL overs) was deagglomerated using a roll crusher having a corru ⁇ gated surface and a gap width of 0.85 mm (deagglomerated SXL polymer).
  • the SXL polymer and the deagglomerated SXL polymer were combined (SXL product).
  • the deagglomerated SXL polymer was screened off to a particle size fraction of 150 to 850 ⁇ and analysed. The results are shown in table 1.
  • Example 1 was repeated, The SXL overs were deagglomerated using a roll crusher having a corrugated surface and a gap width of 1.00 mm. The deagglomerated SXL polymer was screened off to a particle size fraction of 150 to 850 ⁇ and analysed. The results are shown in table 1.
  • Example 3 Example 1 was repeated. The SXL overs were deagglomerated using a roll crusher having a corrugated surface and a gap width of 1.20 mm. The deagglomerated SXL polymer was screened off to a particle size fraction of 150 to 850 ⁇ and analysed. The results are shown in table 1.
  • Example 1 was repeated.
  • the SXL overs were deagglomerated using a rotor mill having a rotor-ring sieve system having round-shaped holes of 10 mm as grinding space bound.
  • the deagglomerated SXL polymer was screened off to a particle size fraction of 150 to 850 ⁇ and analysed. The results are shown in table 1.
  • Example 1 was repeated.
  • the SXL overs were deagglomerated using a rotor mill having a rotor-ring sieve system having round-shaped holes of 6 mm as grinding space bound.
  • the deagglomerated SXL polymer was screened off to a particle size fraction of 150 to 850 ⁇ and analysed. The results are shown in table 1.
  • Tab. 1 Properties of the deagglomerated SXL overs

Landscapes

  • Chemical & Material Sciences (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Dispersion Chemistry (AREA)
  • Engineering & Computer Science (AREA)
  • Food Science & Technology (AREA)
  • Addition Polymer Or Copolymer, Post-Treatments, Or Chemical Modifications (AREA)
  • Processes Of Treating Macromolecular Substances (AREA)
PCT/EP2018/068326 2017-07-12 2018-07-06 PROCESS FOR PRODUCING SUPERABSORBENT POLYMER PARTICLES Ceased WO2019011793A1 (en)

Priority Applications (5)

Application Number Priority Date Filing Date Title
CN201880044601.9A CN110832011B (zh) 2017-07-12 2018-07-06 制备超吸收性聚合物颗粒的方法
JP2020501118A JP7229987B2 (ja) 2017-07-12 2018-07-06 超吸収性ポリマー粒子の製造方法
KR1020207000175A KR102563402B1 (ko) 2017-07-12 2018-07-06 고흡수성 중합체 입자 제조 방법
US16/628,689 US11680142B2 (en) 2017-07-12 2018-07-06 Process for producing superabsorbent polymer particles
EP18734837.0A EP3652237B1 (en) 2017-07-12 2018-07-06 Process for producing superabsorbent polymer particles

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
EP17180871.0 2017-07-12
EP17180871 2017-07-12

Publications (1)

Publication Number Publication Date
WO2019011793A1 true WO2019011793A1 (en) 2019-01-17

Family

ID=59350668

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/EP2018/068326 Ceased WO2019011793A1 (en) 2017-07-12 2018-07-06 PROCESS FOR PRODUCING SUPERABSORBENT POLYMER PARTICLES

Country Status (7)

Country Link
US (1) US11680142B2 (enExample)
EP (1) EP3652237B1 (enExample)
JP (1) JP7229987B2 (enExample)
KR (1) KR102563402B1 (enExample)
CN (1) CN110832011B (enExample)
TW (1) TWI781194B (enExample)
WO (1) WO2019011793A1 (enExample)

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US11958925B2 (en) 2020-02-20 2024-04-16 Upl Ltd Process for preparation of superabsorbent polymer
WO2024115160A1 (de) * 2022-11-29 2024-06-06 Basf Se Verfahren zur herstellung von farbstabilen superabsorberpartikeln
WO2024115158A1 (de) * 2022-11-29 2024-06-06 Basf Se Verfahren zur herstellung von farbstabilen superabsorberpartikeln

Families Citing this family (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN116635154A (zh) * 2021-07-12 2023-08-22 株式会社Lg化学 用于超吸收性聚合物的辊磨机和使用其制备超吸收性聚合物的方法
CN120476171A (zh) * 2023-01-05 2025-08-12 巴斯夫欧洲公司 制备超级吸收剂的方法

Citations (47)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0083022A2 (en) 1981-12-30 1983-07-06 Seitetsu Kagaku Co., Ltd. Water-absorbent resin having improved water-absorbency and improved water-dispersibility and process for producing same
DE3314019A1 (de) 1982-04-19 1984-01-12 Nippon Shokubai Kagaku Kogyo Co. Ltd., Osaka Absorbierender gegenstand
DE3523617A1 (de) 1984-07-02 1986-01-23 Nippon Shokubai Kagaku Kogyo Co. Ltd., Osaka Wasserabsorbierendes mittel
DE3713601A1 (de) 1987-04-23 1988-11-10 Stockhausen Chem Fab Gmbh Verfahren zur herstellung eines stark wasserabsorbierenden polymerisats
DE3825366A1 (de) 1987-07-28 1989-02-09 Dai Ichi Kogyo Seiyaku Co Ltd Verfahren zur kontinuierlichen herstellung eines acrylpolymergels
WO1990015830A1 (en) 1989-06-12 1990-12-27 Weyerhaeuser Company Hydrocolloid polymer
DE4020780C1 (enExample) 1990-06-29 1991-08-29 Chemische Fabrik Stockhausen Gmbh, 4150 Krefeld, De
EP0450922A2 (en) 1990-04-02 1991-10-09 Nippon Shokubai Kagaku Kogyo Co. Ltd. Method for production of fluid stable aggregate
EP0530438A1 (en) 1991-09-03 1993-03-10 Hoechst Celanese Corporation A superabsorbent polymer having improved absorbency properties
EP0543303A1 (de) 1991-11-22 1993-05-26 Hoechst Aktiengesellschaft Hydrophile, hochquellfähige Hydrogele
EP0547847A1 (en) 1991-12-18 1993-06-23 Nippon Shokubai Co., Ltd. Process for producing water-absorbent resin
EP0559476A1 (en) 1992-03-05 1993-09-08 Nippon Shokubai Co., Ltd. Method for the production of absorbent resin
WO1993021237A1 (en) 1992-04-16 1993-10-28 The Dow Chemical Company Crosslinked hydrophilic resins and method of preparation
EP0632068A1 (en) 1993-06-18 1995-01-04 Nippon Shokubai Co., Ltd. Process for preparing absorbent resin
EP0640330A1 (en) 1993-06-30 1995-03-01 The Procter & Gamble Company Hygienic absorbent articles
DE19543368A1 (de) 1995-11-21 1997-05-22 Stockhausen Chem Fab Gmbh Wasserabsorbierende Polymere mit verbesserten Eigenschaften, Verfahren zu deren Herstellung und deren Verwendung
DE19646484A1 (de) 1995-11-21 1997-05-22 Stockhausen Chem Fab Gmbh Flüssigkeitsabsorbierende Polymere, Verfahren zu deren Herstellung und deren Verwendung
DE19807992C1 (de) 1998-02-26 1999-07-15 Clariant Gmbh Verfahren zur Vernetzung von Hydrogelen mit Bis- und Poly-2-oxazolidinonen
EP0937736A2 (en) 1998-02-24 1999-08-25 Nippon Shokubai Co., Ltd. Crosslinking a water-absorbing agent
DE19807502A1 (de) 1998-02-21 1999-09-16 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit 2-Oxazolidinonen
DE19854574A1 (de) 1998-11-26 2000-05-31 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit N-Acyl-2-Oxazolidinonen
DE19854573A1 (de) 1998-11-26 2000-05-31 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit 2-Oxo-tetrahydro-1,3-oxazinen
US6239230B1 (en) 1999-09-07 2001-05-29 Bask Aktiengesellschaft Surface-treated superabsorbent polymer particles
WO2001038402A1 (de) 1999-11-20 2001-05-31 Basf Aktiengesellschaft Verfahren zur kontinuierlichen herstellung von vernetzten feinteiligen gelförmigen polymerisaten
US6241928B1 (en) 1998-04-28 2001-06-05 Nippon Shokubai Co., Ltd. Method for production of shaped hydrogel of absorbent resin
EP1199327A2 (en) 2000-10-20 2002-04-24 Nippon Shokubai Co., Ltd. Water-absorbing agent and process for producing the same
WO2002032962A2 (en) 2000-10-20 2002-04-25 Millennium Pharmaceuticals, Inc. Compositions of human proteins and method of use thereof
WO2002055469A1 (de) 2001-01-12 2002-07-18 Degussa Ag Kontinuierliches verfahren zur herstellung und aufreinigung von (meth) acrylsäure
WO2003031482A1 (de) 2001-10-05 2003-04-17 Basf Aktiengesellschaft Verfahren zur vernetzung von hydrogelen mit morpholin-2,3-dionen
DE10204938A1 (de) 2002-02-07 2003-08-21 Stockhausen Chem Fab Gmbh Verfahren zur Nachvernetzung im Bereich der Oberfläche von wasserabsorbierenden Polymeren mit beta-Hydroxyalkylamiden
DE10204937A1 (de) 2002-02-07 2003-08-21 Stockhausen Chem Fab Gmbh Verfahren zur Nachvernetzung im Bereich der Oberfläche von wasserabsorbierenden Polymeren mit Harnstoffderivaten
WO2003078378A1 (de) 2002-03-15 2003-09-25 Stockhausen Gmbh (meth)acrylsäurekristall und verfahren zur herstellung und aufreinigung von wässriger (meth)acrylsäure
WO2003104299A1 (de) 2002-06-11 2003-12-18 Basf Aktiengesellschaft Verfahren zur herstellung von estern von polyalkoholen
WO2003104300A1 (de) 2002-06-01 2003-12-18 Basf Aktiengesellschaft (meth)acrylester von polyalkoxyliertem trimethylolpropan
WO2003104301A1 (de) 2002-06-11 2003-12-18 Basf Aktiengesellschaft (meth)acrylester von polyalkoxyliertem glycerin
WO2004035514A1 (de) 2002-10-10 2004-04-29 Basf Aktiengesellschaft Verfahren zur herstellung von acrylsäure
US20040242761A1 (en) 2003-05-27 2004-12-02 Yorimichi Dairoku Method for sizing of water-absorbent resin
DE10331450A1 (de) 2003-07-10 2005-01-27 Basf Ag (Meth)acrylsäureester monoalkoxilierter Polyole und deren Herstellung
DE10334584A1 (de) 2003-07-28 2005-02-24 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit bicyclischen Amidacetalen
DE10331456A1 (de) 2003-07-10 2005-02-24 Basf Ag (Meth)acrylsäureester alkoxilierter ungesättigter Polyolether und deren Herstellung
DE10355401A1 (de) 2003-11-25 2005-06-30 Basf Ag (Meth)acrylsäureester ungesättigter Aminoalkohole und deren Herstellung
WO2008037673A1 (de) 2006-09-25 2008-04-03 Basf Se Verfahren zum klassieren wasserabsorbierender polymerpartikel
WO2008040715A2 (de) 2006-10-05 2008-04-10 Basf Se Verfahren zur herstellung wasserabsorbierender polymerpartikel durch polymerisation von tropfen einer monomerlösung
WO2008052971A1 (de) 2006-10-31 2008-05-08 Basf Se Regelung eines verfahrens zur herstellung wasserabsorbierender polymerpartikel in einer erwärmten gasphase
US20120283401A1 (en) * 2011-05-06 2012-11-08 Basf Se Process For Producing Water-Absorbing Polymer Particles
WO2015163512A1 (en) * 2014-04-25 2015-10-29 Songwon Industrial Co., Ltd. Multi-stage milling in the production of water-absorbent polymer particles
WO2016159144A1 (ja) * 2015-04-02 2016-10-06 株式会社日本触媒 ポリアクリル酸(塩)系吸水性樹脂を主成分とする粒子状吸水剤の製造方法

Family Cites Families (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2011025012A1 (ja) * 2009-08-28 2011-03-03 株式会社日本触媒 吸水性樹脂の製造方法
EP2615120B2 (en) * 2012-01-12 2022-12-21 Evonik Superabsorber GmbH Process for the continuous preparation of water-absorbent polymers
US9840598B2 (en) * 2012-07-03 2017-12-12 Basf Se Method for producing water-absorbent polymer particles with improved properties
CN104603159B (zh) * 2012-08-29 2017-07-14 巴斯夫欧洲公司 制备吸水性聚合物颗粒的方法
JP6590800B2 (ja) * 2013-10-30 2019-10-16 ビーエーエスエフ ソシエタス・ヨーロピアBasf Se 吸収性ポリマー粒子を懸濁重合によって製造する方法
JP6913107B2 (ja) * 2016-11-16 2021-08-04 株式会社日本触媒 吸水性樹脂粉末の製造方法及びその製造装置

Patent Citations (48)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0083022A2 (en) 1981-12-30 1983-07-06 Seitetsu Kagaku Co., Ltd. Water-absorbent resin having improved water-absorbency and improved water-dispersibility and process for producing same
DE3314019A1 (de) 1982-04-19 1984-01-12 Nippon Shokubai Kagaku Kogyo Co. Ltd., Osaka Absorbierender gegenstand
DE3523617A1 (de) 1984-07-02 1986-01-23 Nippon Shokubai Kagaku Kogyo Co. Ltd., Osaka Wasserabsorbierendes mittel
DE3713601A1 (de) 1987-04-23 1988-11-10 Stockhausen Chem Fab Gmbh Verfahren zur herstellung eines stark wasserabsorbierenden polymerisats
DE3825366A1 (de) 1987-07-28 1989-02-09 Dai Ichi Kogyo Seiyaku Co Ltd Verfahren zur kontinuierlichen herstellung eines acrylpolymergels
WO1990015830A1 (en) 1989-06-12 1990-12-27 Weyerhaeuser Company Hydrocolloid polymer
EP0450922A2 (en) 1990-04-02 1991-10-09 Nippon Shokubai Kagaku Kogyo Co. Ltd. Method for production of fluid stable aggregate
DE4020780C1 (enExample) 1990-06-29 1991-08-29 Chemische Fabrik Stockhausen Gmbh, 4150 Krefeld, De
EP0530438A1 (en) 1991-09-03 1993-03-10 Hoechst Celanese Corporation A superabsorbent polymer having improved absorbency properties
EP0543303A1 (de) 1991-11-22 1993-05-26 Hoechst Aktiengesellschaft Hydrophile, hochquellfähige Hydrogele
EP0547847A1 (en) 1991-12-18 1993-06-23 Nippon Shokubai Co., Ltd. Process for producing water-absorbent resin
EP0559476A1 (en) 1992-03-05 1993-09-08 Nippon Shokubai Co., Ltd. Method for the production of absorbent resin
WO1993021237A1 (en) 1992-04-16 1993-10-28 The Dow Chemical Company Crosslinked hydrophilic resins and method of preparation
EP0632068A1 (en) 1993-06-18 1995-01-04 Nippon Shokubai Co., Ltd. Process for preparing absorbent resin
EP0640330A1 (en) 1993-06-30 1995-03-01 The Procter & Gamble Company Hygienic absorbent articles
DE19543368A1 (de) 1995-11-21 1997-05-22 Stockhausen Chem Fab Gmbh Wasserabsorbierende Polymere mit verbesserten Eigenschaften, Verfahren zu deren Herstellung und deren Verwendung
DE19646484A1 (de) 1995-11-21 1997-05-22 Stockhausen Chem Fab Gmbh Flüssigkeitsabsorbierende Polymere, Verfahren zu deren Herstellung und deren Verwendung
DE19807502A1 (de) 1998-02-21 1999-09-16 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit 2-Oxazolidinonen
EP0937736A2 (en) 1998-02-24 1999-08-25 Nippon Shokubai Co., Ltd. Crosslinking a water-absorbing agent
DE19807992C1 (de) 1998-02-26 1999-07-15 Clariant Gmbh Verfahren zur Vernetzung von Hydrogelen mit Bis- und Poly-2-oxazolidinonen
US6241928B1 (en) 1998-04-28 2001-06-05 Nippon Shokubai Co., Ltd. Method for production of shaped hydrogel of absorbent resin
DE19854573A1 (de) 1998-11-26 2000-05-31 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit 2-Oxo-tetrahydro-1,3-oxazinen
DE19854574A1 (de) 1998-11-26 2000-05-31 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit N-Acyl-2-Oxazolidinonen
US6239230B1 (en) 1999-09-07 2001-05-29 Bask Aktiengesellschaft Surface-treated superabsorbent polymer particles
WO2001038402A1 (de) 1999-11-20 2001-05-31 Basf Aktiengesellschaft Verfahren zur kontinuierlichen herstellung von vernetzten feinteiligen gelförmigen polymerisaten
EP1199327A2 (en) 2000-10-20 2002-04-24 Nippon Shokubai Co., Ltd. Water-absorbing agent and process for producing the same
WO2002032962A2 (en) 2000-10-20 2002-04-25 Millennium Pharmaceuticals, Inc. Compositions of human proteins and method of use thereof
WO2002055469A1 (de) 2001-01-12 2002-07-18 Degussa Ag Kontinuierliches verfahren zur herstellung und aufreinigung von (meth) acrylsäure
WO2003031482A1 (de) 2001-10-05 2003-04-17 Basf Aktiengesellschaft Verfahren zur vernetzung von hydrogelen mit morpholin-2,3-dionen
DE10204938A1 (de) 2002-02-07 2003-08-21 Stockhausen Chem Fab Gmbh Verfahren zur Nachvernetzung im Bereich der Oberfläche von wasserabsorbierenden Polymeren mit beta-Hydroxyalkylamiden
DE10204937A1 (de) 2002-02-07 2003-08-21 Stockhausen Chem Fab Gmbh Verfahren zur Nachvernetzung im Bereich der Oberfläche von wasserabsorbierenden Polymeren mit Harnstoffderivaten
WO2003078378A1 (de) 2002-03-15 2003-09-25 Stockhausen Gmbh (meth)acrylsäurekristall und verfahren zur herstellung und aufreinigung von wässriger (meth)acrylsäure
WO2003104300A1 (de) 2002-06-01 2003-12-18 Basf Aktiengesellschaft (meth)acrylester von polyalkoxyliertem trimethylolpropan
WO2003104299A1 (de) 2002-06-11 2003-12-18 Basf Aktiengesellschaft Verfahren zur herstellung von estern von polyalkoholen
WO2003104301A1 (de) 2002-06-11 2003-12-18 Basf Aktiengesellschaft (meth)acrylester von polyalkoxyliertem glycerin
WO2004035514A1 (de) 2002-10-10 2004-04-29 Basf Aktiengesellschaft Verfahren zur herstellung von acrylsäure
US20040242761A1 (en) 2003-05-27 2004-12-02 Yorimichi Dairoku Method for sizing of water-absorbent resin
DE10331456A1 (de) 2003-07-10 2005-02-24 Basf Ag (Meth)acrylsäureester alkoxilierter ungesättigter Polyolether und deren Herstellung
DE10331450A1 (de) 2003-07-10 2005-01-27 Basf Ag (Meth)acrylsäureester monoalkoxilierter Polyole und deren Herstellung
DE10334584A1 (de) 2003-07-28 2005-02-24 Basf Ag Verfahren zur Nachvernetzung von Hydrogelen mit bicyclischen Amidacetalen
DE10355401A1 (de) 2003-11-25 2005-06-30 Basf Ag (Meth)acrylsäureester ungesättigter Aminoalkohole und deren Herstellung
WO2008037673A1 (de) 2006-09-25 2008-04-03 Basf Se Verfahren zum klassieren wasserabsorbierender polymerpartikel
WO2008040715A2 (de) 2006-10-05 2008-04-10 Basf Se Verfahren zur herstellung wasserabsorbierender polymerpartikel durch polymerisation von tropfen einer monomerlösung
WO2008052971A1 (de) 2006-10-31 2008-05-08 Basf Se Regelung eines verfahrens zur herstellung wasserabsorbierender polymerpartikel in einer erwärmten gasphase
US20120283401A1 (en) * 2011-05-06 2012-11-08 Basf Se Process For Producing Water-Absorbing Polymer Particles
WO2015163512A1 (en) * 2014-04-25 2015-10-29 Songwon Industrial Co., Ltd. Multi-stage milling in the production of water-absorbent polymer particles
WO2016159144A1 (ja) * 2015-04-02 2016-10-06 株式会社日本触媒 ポリアクリル酸(塩)系吸水性樹脂を主成分とする粒子状吸水剤の製造方法
EP3279239A1 (en) * 2015-04-02 2018-02-07 Nippon Shokubai Co., Ltd. Method for producing particulate water-absorbing agent that has polyacrylic acid (salt)-based water-absorbing resin as main component

Non-Patent Citations (2)

* Cited by examiner, † Cited by third party
Title
"Perry's Chemical Engineer's Handbook", MCGRAW-HILL BOOK GROUP, pages: 8 - 26,8-27
F.L. BUCHHOLZ; A.T. GRAHAM: "Modern Superabsorbent Polymer Technology", 1998, WILEY-VCH, pages: 71 - 103

Cited By (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US11958925B2 (en) 2020-02-20 2024-04-16 Upl Ltd Process for preparation of superabsorbent polymer
WO2024115160A1 (de) * 2022-11-29 2024-06-06 Basf Se Verfahren zur herstellung von farbstabilen superabsorberpartikeln
WO2024115158A1 (de) * 2022-11-29 2024-06-06 Basf Se Verfahren zur herstellung von farbstabilen superabsorberpartikeln

Also Published As

Publication number Publication date
TW201908374A (zh) 2019-03-01
US20200216622A1 (en) 2020-07-09
KR20200030047A (ko) 2020-03-19
JP7229987B2 (ja) 2023-02-28
US11680142B2 (en) 2023-06-20
EP3652237B1 (en) 2022-01-19
CN110832011B (zh) 2023-03-10
KR102563402B1 (ko) 2023-08-04
JP2020526633A (ja) 2020-08-31
TWI781194B (zh) 2022-10-21
CN110832011A (zh) 2020-02-21
EP3652237A1 (en) 2020-05-20

Similar Documents

Publication Publication Date Title
US8410222B2 (en) Method for producing water-absorbing polymer particles
EP2890722B1 (en) Process for producing water-absorbing polymer particles
US20090318633A1 (en) Process for Continuously Producing Water-Absorbing Polymer Particles
US11680142B2 (en) Process for producing superabsorbent polymer particles
US8420773B2 (en) Process for producing water-absorbing polymer particles
US20110204288A1 (en) Process for Producing Water-Absorbing Polymer Particles
KR102528637B1 (ko) 초흡수제의 제조 방법
EP3661662B1 (en) Classification process for superabsorbent polymer particles
CN103502324B (zh) 制备吸水聚合物颗粒的方法
EP2890411B1 (en) Process for producing water-absorbing polymer particles
EP3931239B1 (en) Process for producing superabsorbent polymer particles
US12084527B2 (en) Method for producing super absorber particles
CN116568732A (zh) 制备超吸收剂颗粒的方法

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 18734837

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2020501118

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 2018734837

Country of ref document: EP

Effective date: 20200212