WO2012033988A1 - Technique for manufacturing bit patterned media - Google Patents

Technique for manufacturing bit patterned media Download PDF

Info

Publication number
WO2012033988A1
WO2012033988A1 PCT/US2011/050944 US2011050944W WO2012033988A1 WO 2012033988 A1 WO2012033988 A1 WO 2012033988A1 US 2011050944 W US2011050944 W US 2011050944W WO 2012033988 A1 WO2012033988 A1 WO 2012033988A1
Authority
WO
WIPO (PCT)
Prior art keywords
region
intermediate layer
modified region
separator
species
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/US2011/050944
Other languages
English (en)
French (fr)
Inventor
Frank Sinclair
Julian G. Blake
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Varian Semiconductor Equipment Associates Inc
Original Assignee
Varian Semiconductor Equipment Associates Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Varian Semiconductor Equipment Associates Inc filed Critical Varian Semiconductor Equipment Associates Inc
Priority to JP2013528315A priority Critical patent/JP2013537348A/ja
Priority to KR1020137008510A priority patent/KR20130105849A/ko
Priority to CN2011800516274A priority patent/CN103180903A/zh
Publication of WO2012033988A1 publication Critical patent/WO2012033988A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • G—PHYSICS
    • G11—INFORMATION STORAGE
    • G11B—INFORMATION STORAGE BASED ON RELATIVE MOVEMENT BETWEEN RECORD CARRIER AND TRANSDUCER
    • G11B5/00—Recording by magnetisation or demagnetisation of a record carrier; Reproducing by magnetic means; Record carriers therefor
    • G11B5/84—Processes or apparatus specially adapted for manufacturing record carriers
    • G11B5/855—Coating only part of a support with a magnetic layer

Definitions

  • the present application relates to data storage media, particularly to manufacturing a bit patterned media.
  • a bit patterned media which may be the next generation of data storage media, may extend the data storage capacity of hard drive disks.
  • BPM may include a base 102, a storage layer 104, an intermediate layer 103, and a protective layer 106.
  • Within the data storage layer 104 there may be a plurality of active regions 104b, each of which is used for storing a single bit of data, and one or more separators 104a for isolating each active region 104b.
  • the capacity of the media 100 depends on the number of the active regions 104b.
  • a media 100 with greater number of active regions 104b may store more data.
  • the active regions are formed during manufacturing of the media 100. This is contrary to earlier data storage media, where the active regions are formed while the data is recorded. Referring to FIG. la- If, there is shown a conventional method for manufacturing BPM 100.
  • the media 100 may comprise a base 102 and the data storage layer 104.
  • the data storage layer 104 may contain ferromagnetic material.
  • a patterning process is performed on the media 100.
  • a layer of resist 108 is deposited onto the data storage layer 104 (FIG. la).
  • the resist layer 108 is patterned using a known lithographic process such as the photolithographic process, the nano- imprint lithographic process, or the direct write electron beam lithographic process.
  • a known lithographic process such as the photolithographic process, the nano- imprint lithographic process, or the direct write electron beam lithographic process.
  • FIG. lb one or more portions of the data storage layer 104 are exposed after the lithographic process.
  • an etching step may be performed.
  • An example of the etching step may be the ion milling process.
  • reactive ions 122 are directed toward the exposed portions of the data storage layer 104, and the ferromagnetic material from the exposed portions is removed (FIG. lc). Meanwhile, portions of the data storage layer 104 that are not exposed are shielded by the resist 106 and remain on the media 100.
  • the resulting media 100 may comprise columns 104b of ferromagnetic material spaced apart and isolated from each other by gaps. The columns that remain on the media 100 may ultimately form the active regions 104b. Areas between the columns (e.g.
  • the resulting media 100 comprises a data storage layer 104 having a plurality of active regions 104b isolated by one or more non- magnetic separators 104a.
  • the resist 108 is deposited on the data storage layer 204 (FIG. 2a).
  • the material in the data storage layer 204 may be ferromagnetic material.
  • the resist layer 108 is patterned using one of the known lithographic processes, and portion(s) of the data storage layer 204 are exposed.
  • ions 222 are directed toward the data storage layer 204. In this process, the ions 222 are implanted into the data storage layer 204.
  • the ions 222 then convert the material in the regions 204a from ferromagnetic material to a material with low permeability and ideally no remanence to form the separators 204a (FIG. 2c).
  • the resulting data storage layer 204 may include active regions 204b, which were not exposed to the ions, and one or more separators 204a formed via exposure to the ions (FIG. 2d).
  • the separators 204b when formed, may isolate each active region 204b.
  • the remaining resist layer 108 is removed, and a protective layer 106 is deposited onto the storage layer 204 (FIG. 2e).
  • the separators 204a are formed via dilution of magnetic material. In this approach, the
  • ferromagnetic material in the exposed regions is implanted with diluting ions, for example ion species that do not exhibit magnetic property, with sufficient dose.
  • diluting ions for example ion species that do not exhibit magnetic property
  • Curie temperature of the resulting material is reduced to room temperature or the material is no longer magnetic at room temperature.
  • atomic concentration of -10% or more of the diluting ions may be needed.
  • a 10% concentration implies an ion dose of approximately 3 x
  • This dose may be proportional to the thickness of the storage layer and thus may be less if the data storage layer is thinner.
  • the magnetic material may be converted by affecting the crystallinity or microstructure of the material in the exposed regions.
  • the ion implantation process is an energetic process that can cause many atomic collisions.
  • the material in the exposed regions that is otherwise crystalline may become amorphous and/or disordered. As a result, the material may exhibit low ferromagnetism at room temperature.
  • the material in the unexposed portions next to the exposed portions may retain its original magnetic property.
  • This approach may be effective if the original ferromagnetic layer is a multilayer that derives its magnetic properties from the interaction of very thin layers in a stack.
  • this approach also may require a high ion dose.
  • a typical ion dose necessary to amorphize/disorder a silicon substrate is IxlO 15 ions/cm 2 or higher. In a metal substrate, this required dose may be even higher, particularly if the implant is performed at room temperature.
  • the beam current in a conventional ion implanter is limited due to the limitations in generating the ions. Accordingly, such a high dose will limit the throughput or increase the time the ion implantation system has to process the media. With limited throughput, the cost associated with manufacturing BPM may be high.
  • the throughput may also be limited in part by the resist patterning step.
  • the electron beam direct write patterning step may be used to pattern the resist. In this process, an electron beam is scanned along one or more directions directly write or pattern the resist. Although this process enables greater resolution, this process is very slow and it is not suitable for high throughput production.
  • the nano-imprint lithography process a more efficient resist patterning process may be used to increase the throughput.
  • This patterning process does not produce resist with desired properties.
  • the maximum practical resist height achieved in the nano- imprint lithography process may be limited to about 50nm.
  • Such resist may not survive the subsequent high dose ion implantation process and/or adequately protect the material underneath.
  • a portion of the resist may sputtered away during ion implantation, and portions of material outside of the exposed region (i.e. material originally under the resist 108) may be implanted with ions and also converted into the separator 204a. Accordingly, less than optimal BPM may result.
  • high dose ion implantation used to form the separator 204a may also contribute to sputtering of the material in the exposed region. This sputtering effect proceeds in proportion to the total dose needed to form the separator 204a. This sputtering effect may result in a non-planar storage layer. Because the BPM manufacturing process that incorporates the ion implantation step is intended to omit the gap filling step (e.g. FIG. Id), excessive non-planarity between the exposed region and the unexposed region may be highly undesirable.
  • a technique for manufacturing bit pattern media is disclosed.
  • the technique may be realized as a method for manufacturing bit pattern media.
  • the method may comprise forming an intermediate layer comprising a modified region and a first region adjacent to one another, where the modified region and the first region may have at least one different property; depositing magnetic species on the first region of the intermediate layer to form an active region; and depositing non-ferromagnetic species on the modified region of the intermediate layer to form a separator,
  • the modified region and the first region may have different structure.
  • the first region may comprise one or more crystals in a preferred orientation and the modified region may be amorphous.
  • the first region may be amorphous and the modified region may comprise one or more crystals.
  • the first region has a plurality of crystals with uniform orientation and the modified region is amorphous.
  • the intermediate layer may have at least one of g, Ta, and Ti.
  • the separator may comprise SiO2.
  • the modified region may have at least one species that is absent in the first region.
  • the modified region and the separator may have at least one species in common.
  • the at least one species in common may be Si.
  • the method may further comprise etching a surface of the intermediate layer prior to the forming the active region and the separator.
  • the modified region of the intermediate layer may be formed by ion implantation.
  • the ion implantation may be performed at an energy of 15 keV or less.
  • the technique may be realized as a method for manufacturing a bit pattern media.
  • the method may comprise forming an intermediate layer that comprises a modified region and a first region adjacent to one another, where the modified region and the first region have at least one different property; depositing magnetic species on the first region of the intermediate layer to form an active region; and depositing non-ferromagnetic species on the modified region of the intermediate layer to form a separator, where the active region and the separator are formed simultaneously.
  • the first region comprises one or more crystals and the modified region is amorphous.
  • the first region comprises one or more crystals in a preferred orientation and the modified region is amorphous
  • the modified region may be formed by ion implantation.
  • the ion implantation may be performed at an energy of 15 keV or less.
  • the modified region and the separator may contain Si.
  • the method may further comprise etching a surface of the intermediate layer prior to the forming the active region and the separator.
  • the first region has a plurality of crystals with uniform orientation and the modified region is amorphous.
  • the technique may be realized with a data storage media.
  • the media may comprise an intermediate layer having a modified region and a plurality of first regions, where the modified region and the first region have at least one different property; an active region formed on the first region of the intermediate layer, the active region containing a magnetic material; and a separator formed on the modified region, the separator contain a non-ferromagnetic material.
  • the intermediate layer may comprise at least one of Mg, Ta, and Ti.
  • the active regions may comprise at least one of Co, Ni, Cr, and Pt.
  • the separator may comprise SiCfe.
  • the modified region and the first region may have different structure.
  • the first region may comprise one or more crystals and the modified region may be amorphous.
  • the modified region and the first region have different species.
  • FIG. la-lf illustrate a conventional technique for manufacturing BPM.
  • FIG. 2a-2e illustrate another conventional technique for manufacturing BPM.
  • FIG. 3a and 3b illustrate an exemplary BPM according to one embodiment of the present disclosure.
  • FIG. 4a-4f illustrate an exemplary technique for manufacturing BPM according to one embodiment of the present disclosure.
  • FIG. 5a-5f illustrate another exemplary technique for manufacturing BPM according to another embodiment of the present disclosure.
  • FIG. 6a-6f illustrate another exemplary technique for manufacturing BPM according to another embodiment of the present disclosure.
  • the techniques may include forming a data storage layer over an intermediate layer that has been selectively processed.
  • Various processes may be used to selectively process the intermediate layer.
  • a particle or ion implantation process may be used.
  • other processes may be used. Examples of other processes that can be used may include a deposition process, a gas immersion laser doping (GILD) process, and a laser or other magnetic wave irradiation process.
  • GILD gas immersion laser doping
  • the present disclosure focuses on the ion implantation process for the purpose of clarity and simplicity. However, those skilled in the art should recognize that the present disclosure is not limited thereto.
  • the system for ion implantation process may be a beam-line ion implantation system; a plasma assisted doping (PLAD) or plasma immersion ion implantation (Pill) system; or any other mass analyzed or non-mass analyzed ion implantation.
  • PLAD plasma assisted doping
  • Pill plasma immersion ion implantation
  • the ions or the particles may be charged or neutral sub-atomic, atomic, or molecular ions or particles.
  • the types or species of the particles that are used during the particle or ion implantation process are not limited to only those types or species described below.
  • the techniques may include one or more processes for etching or depositing materials.
  • various systems may be used.
  • the present disclosure may focus on the sputter deposition or etching system.
  • the media 300 may comprise, among others, a base layer 302, a data storage layer 304, and a protective layer 308.
  • the data storage layer 304 may be disposed above the base layer 302.
  • the base layer 302 may be one or more layers that support the data storage layer 304.
  • the base layer 302 may include a soft underlayer (not shown).
  • the data storage layer 304 may comprise a plurality of active regions 304b, each of which may store a single bit of data. As shown in FIG. 3b, each active region 304b is isolated from one another by a separator 304a.
  • the data storage layer 304 may be a single, continuous separator 304a or a plurality of non- continuous separator segments 304a that surround and magnetically decouple each active region 304b.
  • the BPM 300 may also include an intermediate layer 303.
  • the intermediate layer 303 may be separate from the base layer 302.
  • the intermediate layer 303 may be a part of the base layer 302 or one of the layers that form the base layer 302.
  • the intermediate layer 303 of the present embodiment may optionally contain a modified region 303a. If the intermediate layer 303 contains the modified region 303a, the region outside the modified region 303a, for the purpose of clarity and simplicity, may be a first region 303b. In the present embodiment, the separator 304a may be disposed on the modified region 303a, whereas the active region 304b may be disposed on the first region 303b. In another embodiment, the separator 304a may be disposed on the first region 303b, whereas the active region 304b may be disposed on the modified region 303a.
  • the modified region 303a may have at least one property different from the first region 303b.
  • the modified region 303a and the first region 303b may have different structure and/or crystal orientation.
  • one of the modified region 303a and the first region 303b may have a plurality of crystals, whereas the other one of the modified region 303a and the first region 303 may be amorphous.
  • one of the modified region 303a and the first region 303b may have crystals or seeds with a preferred orientation that may act as a template for expitaxial growth of the active regions 304b.
  • the other one of the modified region 303a and the first region 303b may be amorphous or substantially without crystals with preferred orientation.
  • the preferred orientation may be one or more orientations that enable or promote epitaxial formation of the active region 304b.
  • a region without the crystals having preferred orientation may be either amorphous or may have crystals that do not act as template for expitaxial growth of the active regions 304b.
  • the crystals with preferred orientation may have orientation that is identical to the orientation of the crystals in the active region 304b. In some other embodiments, the crystals with preferred orientation may have uniform orientation.
  • modified region 303a may be in the difference of the species.
  • the modified region 303a may contain one or more species that are not contained in the first region 303b.
  • the intermediate layer 303 may preferably comprise titanium (Ti), magnesium (Mg), or tantalum (Ta) based material containing at least one Ti, Mg, and Ta species.
  • the intermediate layer 303 may contain Ti species.
  • the intermediate layer 303 may be magnesium oxide (MgO) containing Mg species.
  • MgO magnesium oxide
  • the separator 304a may preferably be non-ferromagnetic with low permeability and remanence.
  • non-ferromagnetic material may include paramagnetic material, ferrimagnetic material, antiferromagnetic material, and any other non- ferromagnetic or non-magnetic material.
  • the separator 304a of the present embodiment may be silicon dioxide (SiO?.) containing at least silicon (Si) and oxygen (0) species.
  • the separator 304b may be other non-ferromagnetic material containing other species.
  • the active regions 304b of the present embodiment may contain one or more magnetic materials, in one or more layers.
  • the active regions 304b are preferably ferromagnetic material.
  • the species that may contain in the active region 304a may be at least one of cobalt (Co), nickel (Ni), chromium (Cr), and platinum (Pt) species.
  • the active regions 304b with other magnetic or ferromagnetic material with high permeability and remanence are not precluded in the present disclosure.
  • the active regions 304b When viewed from the top, the active regions 304b may be substantially circular or having a curved boundary (FIG. 3b).
  • the diameter or the cross-sectional thickness (when viewed from the top) of the active region 304b may range between about 5 nm to about 10 nm.
  • the separator 304a which may surround each active region 304b, may have a cross sectional thickness ranging about 1 nm to about 4 nm (FIG. 3b). Such a thickness range is preferred as it may magnetically decouple the neighboring active regions 304b to hinder the spin direction therein from affecting one another.
  • the separator 304a with less thickness is not precluded as long as it is capable of sufficiently decoupling the neighboring active regions 304b.
  • the separator 304a with greater thickness, although not precluded, may not be preferred as such a separator 304b may decrease the density or the number of the active regions 304b in the BPM 300.
  • each active region 304b may store a single bit of data. With its active region 304b and the separator 304a, the BPM 300 of the present embodiment may have greater data storage capacity compared to other conventional data storage media.
  • BPM 400 of the present embodiment may comprise, among others, an intermediate layer 403, a data storage layer 404, and a protective layer 406.
  • the data storage layer 404 there may be active regions 404b, each of which is isolated from one another by a separator 404a.
  • the intermediate layer 403 which may or may not be a part of a base layer 402, is prepared (FIG. 4a).
  • the intermediate layer 403 which may or may not be a part of a base layer 402, is prepared (FIG. 4a).
  • intermediate layer 403 may comprise a plurality of crystals or seeds with a preferred orientation. Such an intermediate layer 403 is selectively processed and a portion of the intermediate layer 403 is converted to a modified region 403a.
  • Selective processing of the intermediate layer 403 may be achieved using various processes.
  • a lithographic process that includes resist patterning may be used.
  • a layer of resist 408 may be disposed on the intermediate layer 403 as shown in FIG. 4a.
  • a known patterning process such as electron beam direct write lithography, extreme ultraviolet lithography, or nano-imprint lithography may be used to pattern and expose portion of the intermediate layer 403 (FIG. 4b).
  • the exposed portion of the intermediate layer 403 may then be processed to form the modified region 403a.
  • selective processing of the intermediate layer 403 may be achieved without the lithographic process.
  • a mask may be used to selectively process portion of the intermediate layer 403.
  • a system capable of selectively processing portion of the intermediate layer 403 may be used to form the modified region 403a having desired shape and dimension.
  • the modified region 403a may have at least one property different from the first region 403b or a portion of the intermediate layer 403 that is not exposed.
  • the modified region 403a may be amorphous or substantially without crystals with preferred orientation. This structure may be different from the structure of the first region 403b that contains crystals with preferred orientation
  • An ion implantation process may be performed in the present embodiment to form the modified region 403a. In other embodiments, other processes may be used. In this process, ions or particles 422 may be introduced into the exposed portion of the intermediate layer 403 to amorphize or otherwise alter the orientation of the crystal in the exposed region (FIG. 4c). As such, the modified region 403a may form. In the first region 403b, the crystals with preferred orientation may be maintained.
  • the ions or particles 422 that may be used to form the modified region 403a may include charged or neutral sub-atomic, atomic, or molecular particles or ions.
  • the species of the ions or particles chosen may preferably include hydrogen (H), nitrogen (N), helium (He), neon (Ne), argon (Ar), and krypton (Kr).
  • H hydrogen
  • N nitrogen
  • He helium
  • Ne neon
  • Au argon
  • Kr krypton
  • one or more inert species that do not react readily with the species in the intermediate layer 303 are preferred. However, using one or more reactive species is not precluded in the present disclosure.
  • the ion energy to form the modified region 403a may preferably be low energy, about 15 keV or less. This low energy implantation is preferred as such energy may allow the
  • the resist 408 may be removed after forming the modified region 403a (FIG. 4d).
  • a thorough cleaning of the intermediate layer 403 to remove all traces of the resist 408 is preferred. In some embodiments, even few atomic layers of the intermediate layer 403 may be removed.
  • Example of this optional cleaning process may include an etching (e.g. atomic layer etching) and sputter cleaning process. However, other cleaning or etching processes may also be used.
  • the resulting structure may include the intermediate layer 402 containing the modified region 403a and the first region 403b as shown in FIG. 4d.
  • the data storage layer 404 comprising the separator 404a and the active regions 404b may form.
  • non-ferromagnetic separator 403a for example, SiO2 separator 404a
  • magnetic active regions 404b preferably ferromagnetic active regions 404b
  • the separator 404a and the active region 404b may form simultaneously.
  • the separator 404a and the active regions 404b may form in separate steps, one after another.
  • the species that may ultimately form the active regions 404b and the separator 404a may be simultaneously introduced near the intermediate layer 403.
  • Si and 0, and at least one of Co, Ni, Cr, and Pt may be introduced to form SiO2
  • the separator 504a and active regions 504b containing at least one of Co, Ni, Cr, and Pi may act as a template and the active region 404b may preferentially and heteroepitaxially form over the first region 403b.
  • the modified region 404a having amorphous structure or substantially without crystals with preferred orientation may also act as a template for the separator 404a, and the separator 404a may form over the modified region 403a.
  • the modified region 404a may be amorphous, and amorphous SiO2 separator 404a may form on the modified region 403a.
  • a sputter deposition process may be used to form the separator 404a and the active region 404b. In other embodiments, other types of deposition process may be used. As a result, a data storage layer 404 comprising the separator 404a above the modified region 403a and the active regions above the first regions 403a may form.
  • the protective layer 406 such as, for example, DLC cap layer 406 may be deposited as illustrated in FIG. 4f.
  • an optional post treatment process may be performed.
  • the optional post treatment process may include an annealing process. Sf performed, this optional process may be performed after forming the separator 404a.
  • the BPM 500 of the present embodiment may comprise, among others, an intermediate layer 503, a data storage layer 504, and a protective layer 506.
  • the data storage layer 504 there may be a plurality of active regions 504b, each of which is isolated from one another by a separator 504a.
  • the intermediate layer 503 which may or may not be a part of a base layer 502, is prepared (FIG. 5a).
  • the intermediate layer 503 which may or may not be a part of a base layer 502, is prepared (FIG. 5a).
  • intermediate layer 503 may comprise a plurality of crystals or seeds with a preferred orientation. Such an intermediate layer 503 is selectively processed, and a portion of the intermediate layer 503 is converted to a modified region 503a.
  • Selective processing of the intermediate layer 503 may be achieved using various processes.
  • a iithographic process that includes resist patterning may be used.
  • a layer of resist 508 may be disposed on the intermediate layer 503 as shown in FIG. 5a.
  • a known patterning process such as electron beam direct write lithography, extreme ultraviolet lithography, or nano-imprint lithography may be used to pattern and expose a portion of the intermediate layer 503 (FIG. 5b).
  • the exposed portion of the intermediate layer 503 may then be processed to form the modified region 503a.
  • selective processing of the intermediate layer 503 may be achieved without the iithographic process.
  • a mask may be used to selectively process a portion of the intermediate layer 503.
  • a system capable of selectively processing a portion of the intermediate layer 503 may be used to form the modified region 503a having desired shape and dimension.
  • the modified region 503a may have at least one property that differs from the first region 503b or the portion of the intermediate layer 403 that is not processed.
  • the modified region 503a may contain one or more additional species, if desired, the modified region 503a may also have different structure/crystal orientation.
  • the modified region 503a may be amorphous or substantially without crystals with preferred orientation.
  • An ion implantation process may be used in the present embodiment to introduce additional species, and/or alter the structure/crystal orientation in the exposed region of the intermediate layer 503, to form the modified region 503a.
  • other processes may be used. Examples of other processes may include GILD process, diffusion process, or any other species introducing process.
  • GILD process GILD process
  • diffusion process or any other species introducing process.
  • present embodiment focuses on performing ion implantation process. Those of ordinary skill in the art, however, should recognize that the present disclosure is not limited thereto.
  • the ions or particles 522 that may be used to provide additional species and/or alter the structure/crystal orientation may include charged or neutral sub-atomic, atomic, or molecular particles or ions.
  • the species of the ions or particles chosen may preferably include one or more species that may be contained in the separator 504b.
  • the species that are introduced to form the modified region 503b may include silicon (Si) and/or oxygen (0). Such species may be preferred because such species may enhance the formation of SiO2 separator 503a. If a separator other that SiO2 separator is to be formed, other species may be introduced.
  • other species may also be introduced before, during, or after introduction of the species that may be contained in the separator 504b.
  • Such other species may include H, N, He, Ne, Ar, Kr, or any other species that may alter the structure/crystal orientation in the exposed portion of the intermediate layer 503.
  • the ion energy to form the modified region 403a may preferably be a low energy, about 15 KeV or less. This low energy is advantageous as such energy may allow the concentration of the implanted ions or particles 522 to be the maximum near the surface of the modified region 503a. Moreover, the resist 408 will less likely to be damaged or degraded during this low energy ion implantation step. However, other ion implant energies are not precluded in the present disclosure.
  • the resist 508 may be removed after forming the modified region 503a (FIG. 5d).
  • a thorough cleaning to remove all traces of the resist 508 is preferred, in some embodiments, even few atomic layers of the intermediate layer 503 may be removed.
  • this optional cleaning process may include an etching process (e.g. atomic iayer etching) and a sputter cleaning process. However, other cleaning or etching processes may also be used.
  • the resulting structure may include the base 502 and the intermediate Iayer 503 containing the modified region 503a and the first region 503b, as shown in FIG. 5d.
  • the data storage Iayer 504 comprising the separator 504a and the active regions 504b may form.
  • non-ferromagnetic separator 504a for example, SiO2 separator 504a may form on the modified region 503a.
  • magnetic active regions 504b preferably ferromagnetic active regions 504b, may form on the first region 503b.
  • the separator 504a and the active regions 504b may form simultaneously. In other embodiments, the separator 504a and the active regions 504b may form in separate steps, one after another.
  • the species that ultimately form the separator 504a and the active regions 504b may be introduced simultaneously near the intermediate Iayer 503.
  • Si and 0, and at least one of Co, Ni, Cr, and Pt may be introduced to form SiO2 separator 504a and the active regions 504b containing at least one of Co, Ni, Cr, and Pt.
  • Silicon and oxygen may preferentially deposit over the modified region 503a containing Si and/or 0, and formation of SiO2 separator 504a may occur. If the modified region 503a is also amorphous or substantially without crystals with preferred orientation, the structure may also promote formation of the amorphous SiO2 separator 504a on the modified region 503a.
  • the modified region 503a will not likely to serve as a template for formation of the active region 504b. As such, the active region 504b will not likely to form on the modified region 503a. The active regions 504b will instead likely to heteroepitaxially form on the first region 503b which contain the crystals with a preferred orientation.
  • a deposition process such as sputter deposition process may be used to form the separator 504a and the active regions 504b.
  • other deposition processes may be used.
  • a data storage Iayer 504 comprising the separator 504a above the modified region 503a, and the active regions above the first regions 503a, may form.
  • the protective Iayer 506 such as, for example, DLC cap Iayer 506 may be deposited as illustrated in FIG. 5f.
  • an optional post treatment process may be performed.
  • the optional post treatment process may include an annealing process. If performed, this optional process may be performed after forming the separator 504a.
  • BPM 600 of the present embodiment may comprise an intermediate layer 603, a data storage layer 604, and a protective layer 606.
  • the data storage layer 604 there may be a plurality of active regions 604b, each of which is isolated from one another by a separator 604a.
  • the intermediate layer 603 which may or may not be a part of a base layer 602, is prepared (FIG. 6a).
  • the intermediate layer 603 of the present embodiment may be amorphous or substantially without crystals in preferred orientation.
  • the intermediate layer 603 may not serve as a template for subsequent epitaxial formation of the active regions 604b.
  • Such an intermediate layer 603 is selectively processed, and a portion of the intermediate layer 603 is converted into a plurality of modified regions 603a.
  • Selective process of the intermediate layer 603 may be achieved using various processes.
  • a lithographic process that includes resist patterning may be used.
  • a layer of resist 608 may be disposed on the intermediate layer 603 as shown in FIG. 6a.
  • a known patterning process such as electron beam direct write lithography, extreme ultraviolet lithography, or nano-imprint lithography may be used to pattern and expose a portion of the intermediate layer 603 (FIG. 6b).
  • the exposed portion of the intermediate layer 603 may then be processed to form the modified region 603a.
  • selective processing of the intermediate layer 603 may be achieved without the lithographic process.
  • a mask may be used to selectively process a portion of the intermediate layer 603.
  • a system capable of selectively processing a portion of the intermediate layer 603 may be used to form the modified region 603a having desired shape and dimension.
  • the modified region 603a may have at least one property different from the first region 603b or a portion of the intermediate layer 603 that is not exposed.
  • the modified region 603a may have crystals in the preferred orientation, whereas the first region 603b may be amorphous or substantially without crystals in the preferred orientation.
  • energy 622 in the form of pulsed laser of flash lamp, may be introduced into the exposed portion of the intermediate layer 603 (FIG. 6c).
  • the energy 622 may be introduced via other forms/means including phonons, ions, and other particles.
  • the energy 622 may form the modified regions 603a by altering the structure of the material in the exposed region of the intermediate layer 603.
  • the energy 622 may transform the material in the exposed portion of the intermediate layer from amorphous to crystals in the preferred orientation. Such a transformation may occur with or without melting.
  • additiona! species may also be introduced into the modified region 603a using one of the processes described in earlier embodiments. For example, one of H, N, He, Ne, Ar, Kr, Co, Cr, Ni, and Pt may be introduced. The species may be introduced during the energy 622 introduction step, or before or after.
  • the resist 608 may be removed after forming the modified region 603a (FIG. 6d).
  • a thorough cleaning to remove all traces of the resist 608 is preferred.
  • even few atomic layers of the intermediate layer 603 may be removed. Examples of this optional cleaning process may include an etching process (e.g. atomic layer etching) and a sputter cleaning process. However, other cleaning or etching processes may also be used.
  • the resulting structure may include the intermediate layer 603 containing the modified region 603a and the first region 603b, as shown in FIG. 6d.
  • the data storage layer 604 comprising the separator 604a and the active regions 604b may form.
  • the active regions 604b may form on the modified regions 603a.
  • the separator 604a may form on the first region 603b.
  • each of the processes by which the active regions 604b are formed and by which the separator 604a is formed may be similar to those described in earlier embodiments. As such, detailed description of the formation process will be omitted.
  • the protective layer 606 such as, for example, DLC cap layer 606 may be deposited, as illustrated in FIG. 6f.
  • the process that may be used to form the separator 604a and the active regions 604b may include a sputter deposition process.
  • an optional post treatment process may be performed.
  • the first region 603a may be annealed and converted into one of poly-crystalline or single crystalline structure. If the optional post treatment process is included, the process may be performed after the deposition of the separator 604a.
  • Novel techniques for manufacturing BPM are disclosed.
  • a layer under the data storage layer is processed.
  • the layer is processed prior to formation of the data storage layer.
  • Such embodiments provide several advantages over conventional techniques for manufacturing BPM. Unlike the conventional techniques, planarization might not be necessary after formation of the data storage layer. In addition, lower ion implantation dose and lower energy may be needed. With such advantages, the techniques of the present disclosure may have higher throughput and less costly.

Landscapes

  • Manufacturing Of Magnetic Record Carriers (AREA)
  • Magnetic Record Carriers (AREA)
  • Mram Or Spin Memory Techniques (AREA)
  • Hall/Mr Elements (AREA)
  • Semiconductor Memories (AREA)
PCT/US2011/050944 2010-09-09 2011-09-09 Technique for manufacturing bit patterned media Ceased WO2012033988A1 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
JP2013528315A JP2013537348A (ja) 2010-09-09 2011-09-09 ビット・パターン化媒体を製造する技術
KR1020137008510A KR20130105849A (ko) 2010-09-09 2011-09-09 비트 패터닝된 매체를 제조하기 위한 기술
CN2011800516274A CN103180903A (zh) 2010-09-09 2011-09-09 用于制造位元图案化媒体的技术

Applications Claiming Priority (6)

Application Number Priority Date Filing Date Title
US38128310P 2010-09-09 2010-09-09
US61/381,283 2010-09-09
US38830810P 2010-09-30 2010-09-30
US61/388,308 2010-09-30
US13/228,426 US8709533B2 (en) 2010-09-09 2011-09-08 Technique for manufacturing bit patterned media
US13/228,426 2011-09-08

Publications (1)

Publication Number Publication Date
WO2012033988A1 true WO2012033988A1 (en) 2012-03-15

Family

ID=45807004

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/US2011/050944 Ceased WO2012033988A1 (en) 2010-09-09 2011-09-09 Technique for manufacturing bit patterned media

Country Status (6)

Country Link
US (1) US8709533B2 (enExample)
JP (1) JP2013537348A (enExample)
KR (1) KR20130105849A (enExample)
CN (1) CN103180903A (enExample)
TW (1) TWI488181B (enExample)
WO (1) WO2012033988A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2012094384A1 (en) * 2011-01-04 2012-07-12 Varian Semiconductor Equipment Associates, Inc. Technique for manufacturing bit patterned media

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
SG10201401425RA (en) * 2009-04-13 2014-08-28 Applied Materials Inc Modification of magnetic properties of films using ion and neutral beam implantation

Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0135020A1 (en) * 1983-08-22 1985-03-27 International Business Machines Corporation Magnetic recording disks
JPH01176327A (ja) * 1987-12-29 1989-07-12 Matsushita Electric Ind Co Ltd 垂直磁気記録媒体の製造方法
US20080084635A1 (en) * 2006-10-04 2008-04-10 Samsung Electronics Co., Ltd Magnetic recording medium and method of manufacturing the same
US20090059430A1 (en) * 2007-09-05 2009-03-05 Elizabeth Dobisz Fabricating magnetic recording media on patterned seed layers

Family Cites Families (3)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPWO2005034097A1 (ja) * 2003-09-30 2006-12-14 富士通株式会社 垂直磁気記録媒体、その製造方法、および磁気記憶装置
JP4682721B2 (ja) * 2004-07-07 2011-05-11 富士電機デバイステクノロジー株式会社 垂直磁気記録媒体の製造方法
US8048546B2 (en) * 2009-12-16 2011-11-01 Hitachi Global Storage Technologies Netherlands B.V. Perpendicular magnetic recording disk with ordered nucleation layer and method for making the disk

Patent Citations (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0135020A1 (en) * 1983-08-22 1985-03-27 International Business Machines Corporation Magnetic recording disks
JPH01176327A (ja) * 1987-12-29 1989-07-12 Matsushita Electric Ind Co Ltd 垂直磁気記録媒体の製造方法
US20080084635A1 (en) * 2006-10-04 2008-04-10 Samsung Electronics Co., Ltd Magnetic recording medium and method of manufacturing the same
US20090059430A1 (en) * 2007-09-05 2009-03-05 Elizabeth Dobisz Fabricating magnetic recording media on patterned seed layers

Cited By (2)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO2012094384A1 (en) * 2011-01-04 2012-07-12 Varian Semiconductor Equipment Associates, Inc. Technique for manufacturing bit patterned media
US9093104B2 (en) 2011-01-04 2015-07-28 Varian Semiconductor Equipment Associates, Inc. Technique for manufacturing bit patterned media

Also Published As

Publication number Publication date
KR20130105849A (ko) 2013-09-26
US8709533B2 (en) 2014-04-29
TWI488181B (zh) 2015-06-11
US20120064373A1 (en) 2012-03-15
TW201214426A (en) 2012-04-01
JP2013537348A (ja) 2013-09-30
CN103180903A (zh) 2013-06-26

Similar Documents

Publication Publication Date Title
US8003163B2 (en) Magnetic recording medium and method of manufacturing the same
US6440520B1 (en) Patterned magnetic recording disk with substrate patterned by ion implantation
US8605388B2 (en) Magnetic recording medium with guard layer between auxiliary and magnetic recording layers and manufacturing method of the magnetic recording medium
US9424873B2 (en) Method of manufacturing magnetic recording medium, and magnetic recording medium
JP2009199692A (ja) 磁気記録媒体及びその製造方法
US8679356B2 (en) Mask system and method of patterning magnetic media
WO2003036626A1 (en) Magnetic films having magnetic and non-magnetic regions and method of producing such films by ion irradiation
US8709533B2 (en) Technique for manufacturing bit patterned media
US6180202B1 (en) Large capacity disk and method for manufacturing the same
CN102483929B (zh) 图案化磁性位元数据储存媒体及其制造方法
KR20060056860A (ko) 자기 기록 매체 및 그 제조 방법, 자기 기억 장치, 기판,텍스쳐 형성 장치
KR20010108492A (ko) 데이터 저장용 자기 매체 제조 방법
US9093104B2 (en) Technique for manufacturing bit patterned media
JP4319060B2 (ja) 磁性膜の形成方法、磁性パターンの形成方法及び磁気記録媒体の製造方法
JP2010113773A (ja) 磁気記録媒体およびその製造方法
JP5592630B2 (ja) パターンドメディアの製造方法
US20240185885A1 (en) Method of forming patterned magnetic media
Wodarz et al. Characterization of electrodeposited Co-Pt nanodot array at initial deposition stage
JP2009163819A (ja) 磁気記録媒体の製造方法
KR100803213B1 (ko) 패턴된 자기기록매체 및 그 제조방법
JPH11339241A (ja) 磁気記録媒体および磁気記録媒体の製造方法
JP4319058B2 (ja) 磁性膜の形成方法、磁性パターンの形成方法及び磁気記録媒体の製造方法
JP2000298825A (ja) 磁気記録媒体およびその製造方法
JP2011081873A (ja) 垂直磁気記録媒体用記録層、垂直磁気記録媒体、及び強磁性金属膜の作製方法
Schaub et al. Surface Atomic Scale Engineering by Deposition of Mass Selected Clusters: STM and Helium Scattering Analysis

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 11764892

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 2013528315

Country of ref document: JP

Kind code of ref document: A

NENP Non-entry into the national phase

Ref country code: DE

ENP Entry into the national phase

Ref document number: 20137008510

Country of ref document: KR

Kind code of ref document: A

122 Ep: pct application non-entry in european phase

Ref document number: 11764892

Country of ref document: EP

Kind code of ref document: A1