WO1996027631A1 - Procede de production de solutions de polyolefines - Google Patents

Procede de production de solutions de polyolefines Download PDF

Info

Publication number
WO1996027631A1
WO1996027631A1 PCT/JP1996/000564 JP9600564W WO9627631A1 WO 1996027631 A1 WO1996027631 A1 WO 1996027631A1 JP 9600564 W JP9600564 W JP 9600564W WO 9627631 A1 WO9627631 A1 WO 9627631A1
Authority
WO
WIPO (PCT)
Prior art keywords
liquid supply
kneader
polyolefin resin
polyolefin
liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/JP1996/000564
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
Tetsuro Nogata
Kotaro Takita
Kenji Miyasaka
Koichi Kono
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tonen Chemical Corp
Original Assignee
Tonen Sekiyu Kagaku KK
Tonen Chemical Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tonen Sekiyu Kagaku KK, Tonen Chemical Corp filed Critical Tonen Sekiyu Kagaku KK
Priority to EP96905028A priority Critical patent/EP0774481B1/en
Priority to CA002189868A priority patent/CA2189868C/en
Priority to DE69622665T priority patent/DE69622665T2/de
Priority to US08/737,205 priority patent/US5741848A/en
Publication of WO1996027631A1 publication Critical patent/WO1996027631A1/ja
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J3/00—Processes of treating or compounding macromolecular substances
    • C08J3/02—Making solutions, dispersions, lattices or gels by other methods than by solution, emulsion or suspension polymerisation techniques
    • C08J3/09—Making solutions, dispersions, lattices or gels by other methods than by solution, emulsion or suspension polymerisation techniques in organic liquids
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
    • B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
    • B29C48/00—Extrusion moulding, i.e. expressing the moulding material through a die or nozzle which imparts the desired form; Apparatus therefor
    • B29C48/25—Component parts, details or accessories; Auxiliary operations
    • B29C48/285—Feeding the extrusion material to the extruder
    • B29C48/297—Feeding the extrusion material to the extruder at several locations, e.g. using several hoppers or using a separate additive feeding
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
    • B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
    • B29C48/00—Extrusion moulding, i.e. expressing the moulding material through a die or nozzle which imparts the desired form; Apparatus therefor
    • B29C48/25—Component parts, details or accessories; Auxiliary operations
    • B29C48/36—Means for plasticising or homogenising the moulding material or forcing it through the nozzle or die
    • B29C48/395—Means for plasticising or homogenising the moulding material or forcing it through the nozzle or die using screws surrounded by a cooperating barrel, e.g. single screw extruders
    • B29C48/40—Means for plasticising or homogenising the moulding material or forcing it through the nozzle or die using screws surrounded by a cooperating barrel, e.g. single screw extruders using two or more parallel screws or at least two parallel non-intermeshing screws, e.g. twin screw extruders
    • B—PERFORMING OPERATIONS; TRANSPORTING
    • B29—WORKING OF PLASTICS; WORKING OF SUBSTANCES IN A PLASTIC STATE IN GENERAL
    • B29C—SHAPING OR JOINING OF PLASTICS; SHAPING OF MATERIAL IN A PLASTIC STATE, NOT OTHERWISE PROVIDED FOR; AFTER-TREATMENT OF THE SHAPED PRODUCTS, e.g. REPAIRING
    • B29C48/00—Extrusion moulding, i.e. expressing the moulding material through a die or nozzle which imparts the desired form; Apparatus therefor
    • B29C48/25—Component parts, details or accessories; Auxiliary operations
    • B29C48/36—Means for plasticising or homogenising the moulding material or forcing it through the nozzle or die
    • B29C48/50—Details of extruders
    • B29C48/505—Screws
    • B29C48/625—Screws characterised by the ratio of the threaded length of the screw to its outside diameter [L/D ratio]
    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08J—WORKING-UP; GENERAL PROCESSES OF COMPOUNDING; AFTER-TREATMENT NOT COVERED BY SUBCLASSES C08B, C08C, C08F, C08G or C08H
    • C08J2323/00—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers
    • C08J2323/02—Characterised by the use of homopolymers or copolymers of unsaturated aliphatic hydrocarbons having only one carbon-to-carbon double bond; Derivatives of such polymers not modified by chemical after treatment

Definitions

  • the present invention relates to a method for producing a polyolefin solution used for producing a microporous polyolefin membrane, a polyolefin fiber, and the like. More specifically, the present invention relates to a polyolefin capable of continuously and stably obtaining a high discharge amount of a polyolefin solution having a wide molecular weight distribution. It relates to a method for producing a solution.
  • Polyolefin resin materials have excellent mechanical strength and physical properties and are therefore used for various applications.
  • the polyolefin microporous membrane and microporous fiber are used as separators for batteries, diaphragms for electrolytic capacitors, microfiltration, air filters, and the like.
  • Polyolefin resins are generally produced using a flow improver addition or a polyolefin solution dissolved in a solvent.
  • the polyolefin solution is usually produced by batch kneading or continuous kneading of a polyolefin resin and a liquid such as mineral oil.
  • a polyolefin resin and a liquid such as mineral oil.
  • the polyolefin and the liquid are put into an autoclave equipped with a stirrer, and the temperature is increased while stirring to knead the polyolefin and the liquid.
  • the batch type has a disadvantage that the kneading time is long.
  • the residence time differs between the beginning and the end of taking out of the batch, so that the quality in the batch or at the time of batch switching is unstable, and There are drawbacks such as need. Further, there are problems that a high-viscosity solution cannot be prepared, and a pellet-like polymer composition cannot be used.
  • a continuous kneader provided with a liquid supply section downstream of the resin supply section has been used for producing a polyolefin solution.
  • the internal pressure of the kneading machine in the liquid supply section is high, and the pressure in the liquid supply section is higher than the downstream pressure. Therefore, when the liquid supply amount was increased, the phenomenon that the kneading with the polyolefin became insufficient and the liquid flowed back to the upstream side was observed, and it was necessary to keep the liquid supply amount low.
  • shearing heat is large in a kneader region where only a polymer is present, and thermal degradation occurs.
  • an object of the present invention is to provide a production method capable of continuously and stably obtaining a polyolefin solution at a high discharge rate.
  • the present inventors have found that the continuous kneading machine having a self-cleaning action is used to make the inside of the kneading machine in the polyolefin resin supply section, the liquid supply section and the kneading section starved. As a result, the present inventors have found that a uniform polyolefin solution can be continuously and stably obtained at a high discharge rate, and have reached the present invention.
  • the method for producing a polyolefin solution of the present invention is a method of kneading a polyolefin resin and a liquid comprising the solvent,
  • the method for producing a polyolefin solution of the present invention is a method of kneading a polyolefin resin and a liquid comprising the solvent,
  • At least one liquid supply unit is provided downstream of the polyolefin resin supply unit
  • the kneader internal pressure in at least a part between the polyolefin resin supply unit and the most upstream liquid supply unit is larger than the kneader internal pressure in the most upstream liquid supply unit.
  • FIG. 1 is a schematic view showing a pressure gauge installation position and a liquid supply site in an extruder as a first embodiment of the present invention.
  • FIG. 7 is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a second embodiment of the present invention.
  • FIG. 9 is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a third embodiment of the present invention.
  • FIG. 11 is a schematic view showing a pressure gauge installation position and a liquid supply site in an extruder as a fourth embodiment of the present invention.
  • FIG. 1 It is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a sixth embodiment of the present invention.
  • FIG. 1 It is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a seventh embodiment of the present invention.
  • FIG. 1 It is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as an eighth embodiment of the present invention.
  • FIG. 10 It is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a ninth embodiment of the present invention.
  • FIG. 1 It is a schematic diagram showing a pressure gauge installation position and a liquid supply site in an extruder as a tenth embodiment of the present invention.
  • reference numerals 1 to 14 indicate a pressure gauge
  • reference numeral 20 indicates an extruder
  • reference numeral 21 indicates a polyolefin supply unit
  • reference numeral 22 indicates a liquid supply unit.
  • polystyrene resin examples include crystalline homopolymers, copolymers, and mixtures thereof obtained by polymerizing ethylene, propylene, 1-butene, 4-methyl-1-pentene, 1-1-hexene and the like.
  • copolymer for example, a block copolymer (multi-stage polymer) obtained by sequentially introducing propylene and ethylene into a reactor can be used.
  • polypropylene, polyethylene and their compositions are preferred.
  • the polyolefin may be used in the form of a powder or a pellet.
  • polyolefin resins a polyolefin containing a component having a molecular weight of 1 ⁇ 10 6 or more is preferable.
  • polyolefin resins containing a component having a molecular weight of 1 ⁇ 10 6 or more include crystalline homopolymers obtained by polymerizing ethylene, propylene, 1-butene, 4-methyl-11-pentene, and 1-hexene, and copolymers. Coalescence and mixtures thereof.
  • ultrahigh molecular weight polyethylene containing 5% by weight or more of a component having a molecular weight of 1 ⁇ 10 6 or more is preferable.
  • the polyolefin resin preferably contains an ultrahigh molecular weight component having a molecular weight of 1 ⁇ 10 6 or more (by GPC) in an amount of 5% by weight or more, more preferably 10 to 90% by weight.
  • the preferred molecular weight distribution (weight average molecular weight / number average molecular weight) of the polyolefin resin is 5 to 300. If the component having a molecular weight of 1 ⁇ 10 6 or more is less than 5% by weight, the stretchability of a molded product using this solution is not improved, and a high-strength molded product cannot be obtained.
  • the molecular weight distribution is preferably in the above range for easier solution adjustment.
  • the polyolefin resin may be a reactor blend (multi-stage polyolefin) or a composition comprising two or more polyolefins.
  • a polyethylene containing a component having a molecular weight of 1 ⁇ 10 6 or more by 5% by weight or more and a polyolefin having a molecular weight of 1 ⁇ 10 4 or more and less than 1 ⁇ 10 6 are blended.
  • a composition formed by blending the ultrahigh molecular weight bolylene and the high molecular weight polyethylene is preferable.
  • reactor blend such as molecular weight contained IX 1 0 6 or more ultra-high molecular weight component 5 wt% or more and a molecular weight distribution (weight-average It can be produced by multi-stage polymerization so that the molecular weight (Z number average molecular weight) is 5 to 300.
  • the multistage polymerization method it is preferable to employ a method of producing a high molecular weight portion and a low molecular weight portion by two-stage polymerization.
  • ultra high molecular weight polyolefin fin or the composition rather preferably contains molecular weight 1 X 1 0 6 or more components 5% by weight or more, particularly
  • the ultrahigh molecular weight polyethylene or the composition of the ultrahigh molecular weight polyethylene and the high density polyethylene is particularly preferable as a solution for forming a microporous membrane.
  • additives such as nucleating agents, antioxidants, ultraviolet absorbers, antiblocking agents, pigments, dyes, inorganic fillers, antibacterial agents, deodorants, and far-infrared radiation agents are added to the polyolefin resin as necessary. Can be added.
  • the liquid to be mixed with the polyolefin resin is a low-volatile solvent that is a good solvent for the polyolefin resin, such as non-volatile aliphatic or cyclic solvents such as nonane, decane, decalin, P-xylene, pendecan, dodecane, and liquid paraffin.
  • a hydrocarbon of the formula or a mineral oil fraction having a boiling point corresponding to these can be used.
  • the mixing ratio of the polyolefin resin to the liquid is such that the liquid is 15 to 2000 parts by weight, preferably 20 to 1500 parts by weight, based on 100 parts by weight of the polyolefin resin. If the liquid exceeds 2000 parts by weight, kneading becomes difficult. On the other hand, if the amount of the liquid is less than 15 parts by weight, the viscosity is high, and the liquid is deteriorated due to heat generated by shearing during kneading.
  • the continuous kneader used to produce the polyolefin solution has a self-cleaning action.
  • a self-cleaning action the screw thread of the other screw or the protrusion of the cylinder passes through the screw groove, so that the mixture does not rotate with the screw and the screw thread of the screw or the screw of the reading disk does not rotate. It is possible to feed in a direction according to the combination angle or the like. Therefore, in the case of having a self-cleaning action, it is possible to starve the liquid supply part and the part where the kneading of the polyolefin resin and the liquid is performed first.
  • the self-cleaning action of the kneading machine has a self-cleaning action in all parts of the mixing building It is not necessary that at least a part of the portion where the mixture exists has a self-cleaning action so that the liquid supply part and the part where the kneading of the polyolefin resin and the liquid is first performed are starved. .
  • self-cleaning action of the kneader has need not have a Self cleaning action in all parts of the kneader, so that the pressure of the liquid supply portion is 1 O k gZ cm 2 or less, the presence of the mixture It is sufficient that at least a part of the part to be cleaned has a self-cleaning action.
  • a continuous kneader a twin-screw kneader or a special single-screw kneader is preferable.
  • a co-rotating interlocking twin-screw kneader and a counter-rotating interlocking twin-screw kneader such as a special short-axis kneader such as Bus Co.
  • a co-rotating twin-screw kneader is particularly preferred.
  • At least one liquid supply unit is provided at or downstream of the polyolefin resin supply unit.
  • a liquid is supplied and kneaded in the middle of a kneader containing a polyolefin resin to prepare a polyolefin resin solution having a uniform concentration.
  • the method for producing a polyolefin solution of the present invention includes a method in which a polyolefin resin and a liquid are supplied from the same supply section and a method in which a liquid supply section is provided downstream of the polyolefin resin supply section. Need to be starved. Furthermore, it is necessary to starve the inside of the kneader at the kneading section of the first liquid and the polyolefin resin.
  • the starvation inside the kneader ⁇ state, the space between the cylinder and the screw is polyolefin resin or polyolefin resin and liquid Is a state where there is a space where no mixture exists. Under such starvation, the pressure in the screw length direction becomes zero.
  • a polyolefin resin supply section and a liquid supply section are provided downstream of the polyolefin resin supply section, at least a part of the kneader between the polyolefin resin supply section and the liquid supply section located at the uppermost stream is filled with the polyolefin resin. It is preferable to supply a very large amount of liquid. Thus, even in the case where the upstream portion has a filled state, the pressure of the portion filled with the polyolefin resin alone can be reduced, and deterioration due to heat generation in the portion of the polyolefin resin alone can be prevented.
  • a portion having a pressure higher than the internal pressure of the liquid supply unit is provided upstream of the liquid supply unit located at the uppermost stream in the starved state.
  • the internal pressure of the kneader is set to be higher than the internal pressure of the kneader in the liquid supply section located at the most upstream position. Further, the internal pressure of the kneader in at least a portion between the liquid supply section located at the most upstream side and the next downstream liquid supply section is increased from the immediately downstream of the polyolefin resin supply section to the internal pressure of the kneader in the two liquid supply sections. More preferably, it is set to be larger. Thus, there is an advantage that the liquid supply amount and the discharge amount increase.
  • the above pressure distribution can be achieved by changing operating conditions such as the shape of the screw of the kneader, the liquid supply position, and the number of rotations of the screw.
  • the internal pressure of the kneader is adjusted to a specific distribution.
  • the internal pressure of the mixed-building machine is the average value of the pressure inside the mixed-building machine over a certain period of time, and this fixed time is long enough to cancel the pressure change due to the rotation of the screw of the mixed-building machine.
  • the internal pressure of the kneader in at least a portion between the polyolefin resin supply unit and the liquid supply unit located at the most upstream position is set to be higher than the internal pressure of the kneader at the liquid supply unit located at the most upstream position. That is, a portion having a pressure higher than the internal pressure of the liquid supply unit is provided upstream of the liquid supply unit located at the most upstream. With such a pressure distribution, even if the amount of liquid to be added is increased, the backflow to the upstream can be prevented, and as a result, the discharge amount can be increased.
  • the internal pressure of the kneader at least in part between each liquid supply unit and the supply unit immediately downstream of the liquid supply unit is set to be smaller than the internal pressure of the liquid supply unit immediately downstream. It is preferable to set it to be large. Further, it is more preferable that the kneader internal pressure in at least a part between each liquid supply unit and the supply unit immediately downstream thereof is set to be higher than the internal pressure in the two liquid supply units. Thereby, there is an advantage that the liquid supply amount and the discharge amount increase.
  • kneader pressure in the liquid supply portion located most upstream is preferably set to 1 O k gZc m 2 or less (gauge pressure).
  • the internal pressure of the kneader is kept within the above range, thereby minimizing the portion filled with polyolefin alone. Heat deterioration can be prevented by suppressing shear heat generation.
  • the above pressure distribution can be achieved by changing the shape of the screw of the kneader.
  • the kneading temperature is from the melting point of polyolefin to 250. C is preferable, and in particular, the melting point of polyolefin + 10 ° C to 220 ° C. C is preferred. If the kneading temperature is lower than the melting point of the polyolefin, sufficient kneading cannot be performed, and if it exceeds 250, the polyolefin resin is deteriorated.
  • the polyolefin resin supply section and the liquid supply section and the first kneading The pressure in the liquid supply unit can be reduced to 0 by starving the interior of the kneader in the unit, and a backflow of liquid occurs even if there is no part filled with polyolefin resin alone upstream of the liquid supply unit Thus, a uniform polyolefin solution can be obtained at a high discharge rate without causing the polyolefin solution to flow.
  • the pressure can be reduced, and deterioration due to heat generation in the polyolefin resin alone can be prevented. A large amount of liquid can be supplied.
  • a uniform discharge of the polyolefin solution can be obtained at a high discharge rate by setting the kneader internal pressure to a specific distribution.
  • Table 1 shows the supplied amounts of the liquid to the used polyolefin resin and liquid and to 100 parts by weight of the polyolefin resin.
  • Table 2 shows the amount of liquid supplied from each liquid supply hole (expressed in parts by weight based on 100 parts by weight of polyolefin), the pressure inside the extruder, and operating conditions.
  • the pressure values shown in Table 2 are values when the atmospheric pressure is set to 0 (kg Z cm 2 , gauge pressure). As shown in Table 1, different extruders were used for each example.
  • the extruder After measuring the pressure of the extruder, it is located in the polyolefin resin supply section or the uppermost stream.
  • the pressure gauge in the liquid supply section and the pressure gauge immediately downstream were removed, and several drops of polyolefin resin (PE) pellets were dropped into the hole where the pressure gauge was attached.
  • the PE pellet immediately entered the extruder. Was. Therefore, the positions of the polyolefin supply unit, the liquid supply unit located at the uppermost stream, and the pressure gauge immediately downstream were starved.
  • the screw between the position of the first pressure gauge immediately downstream of the polyolefin supply unit and the position of the most upstream liquid supply unit and the position of the pressure gauge immediately downstream of the polyolefin supply unit knead the polyolefin resin and the liquid.
  • the obtained polyolefin solution was formed into a sheet having a thickness of 2 mm by breath molding. All the obtained sheets showed a good appearance. Further, the sheets were simultaneously biaxially stretched by a batch type rolling mill, but all could be stretched to a magnification of 2 ⁇ 2 or more. Comparative Examples 1 to 6
  • Example 1 Using the same co-rotating intermeshing twin-screw kneader TEX54 as in Example 1, the polyolefin resin of the type and mixing ratio shown in Table 1 and the liquid were kneaded. In addition, the skew shape of the extruder was selected so as to have a desired pressure distribution.
  • a pressure gauge was installed in the same manner as in Example 1. The pressure gauge installation position and liquid supply site are shown in Fig. 1, Fig. 3, Fig. 4 and Fig. 6. Table 1 shows the correspondence between each comparative example and the figure.
  • Table 2 shows the internal pressure and operating conditions of the extruder. As shown in Table 2, in the comparative example, the pressure exceeded 0 at the position of the liquid supply unit located immediately downstream or the most upstream of the polyolefm resin supply unit and the pressure gauge immediately downstream of the liquid supply unit. He was full and was not starving. However, the pressure values shown in Table 2 are values when the atmospheric pressure is set to 0 (kgZc m 2 , gauge pressure). The operating conditions shown in Table 2 are those at the maximum discharge rate at which stable discharge is observed.
  • PE-1 Powder-like polyethylene with a weight average molecular weight of 3.7 x 10 5
  • PE-2 A weight-average molecular weight of 2.0 ⁇ 10 6 powdered PE and a weight-average molecular weight of 3.7 ⁇ 10 5 powdered PE are dry blended in a ratio of 3:14 ( A component having a molecular weight of 1 ⁇ 10 6 or more according to the GPC method 21.6% by weight).
  • PE-3 pellet-like PE having a weight average molecular weight of 3.7 ⁇ 10 5 .
  • PE - 4 weight-average molecular weight 2.
  • PE-5 powdered PE having a weight average molecular weight of 2 x 10 6 .
  • Liquid paraffin the kinematic viscosity at a temperature of 40 ° C is 64 cSt.
  • Example 1 Liquid supply 150 100 80
  • Example 2 Liquid supply ⁇ 30 150 100 40
  • Liquid supply 50 180 270 150 350 100
  • Liquid supply 80 180 240 150 350 60
  • Example 5
  • Liquid supply allocation 150 150 200 100 Example 7
  • the screw shape of the extruder was selected so as to have a desired pressure distribution.
  • 14 pressure gauges were installed inside the kneader.
  • Figures 7 to 10 show the pressure gauge installation positions and liquid supply sites inside the extruder.
  • Tables 4 and 6 show the correspondence between the examples and the figures. However, the distance from the pressure gauge 1 to the left end of the extruder 20 was 142 mm, and the distance between each adjacent pressure gauge was 94.5 mm.
  • the operating conditions are shown in Tables 4 and 6, and the measured pressure distributions are shown in Tables 5 and 7. However, the pressure values shown in Tables 5 and 7 are values (gauge pressure) when the atmospheric pressure is set to 0. The operating conditions shown in Tables 4 and 6 are at the maximum discharge rate at which stable discharge is observed.
  • the obtained polyolefin solution was directly molded into a sheet having a thickness of 2 mm by press molding. All the obtained sheets showed a good appearance. Although the sheets were simultaneously biaxially stretched by a batch rolling mill, they could all be stretched to a magnification of 2 X 2 or more.
  • Example 17 Using the same co-rotating intermeshing twin-screw kneader TEX54 as in Example 17, polyolefin resins of the types and compounding ratios shown in Table 3 and the liquid were kneaded. The screw shape of the extruder was selected so as to obtain a desired pressure distribution. A pressure gauge was installed in the same manner as in Example 17. Figures 7 to 10 show the pressure gauge installation positions and liquid supply sites. Tables 4 and 6 show the correspondence between the comparative examples and the figures.
  • the operating conditions are shown in Tables 4 and 6, and the measured pressure distributions are shown in Tables 5 and 7. However, the pressure values shown in Tables 5 and 7 are values (gauge pressure) when the atmospheric pressure is set to 0. The operating conditions shown in Tables 4 and 6 are at the maximum discharge rate at which stable discharge is observed.
  • Comparative Examples 7, 8, 10, 10 and 11 when the discharge amount was increased, the fluctuation became severe, and a phenomenon was observed in which the unmixed liquid was discharged periodically. Further, the polyolefin solutions of Comparative Examples 9 and 12 were directly formed into a sheet having a thickness of 2 mm by press molding, and the sheets were simultaneously biaxially stretched by a batch stretching machine, but were broken under any conditions. Table 3
  • Liquid supply Expressed as parts by weight of liquid per 100 parts by weight of polyolefin resin.
  • Liquid supply amount Expressed as parts by weight of liquid per 100 parts by weight of polyolefin resin.
  • the method of the present invention prevents the liquid from flowing backward by starvating the inside of the kneader at the polyolefin resin supply section, the liquid supply section, and the first kneading section, thereby forming a uniform polyolefin solution. It can be obtained continuously and with a high discharge rate.
  • the polyolefin solution obtained by such a method of the present invention can be used for producing various polyolefin molded articles.
  • the method of the present invention can prevent the liquid from flowing back by setting the pressure in the kneader to a specific distribution, so that a uniform polyolefin solution can be obtained continuously and at a high discharge rate.
  • the polyolefin solution obtained by the method of the present invention can be used for producing various polyolefin molded articles, but is particularly useful for forming a microporous membrane.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Dispersion Chemistry (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Organic Chemistry (AREA)
  • Processing And Handling Of Plastics And Other Materials For Molding In General (AREA)
  • Compositions Of Macromolecular Compounds (AREA)
  • Processes Of Treating Macromolecular Substances (AREA)
PCT/JP1996/000564 1995-03-08 1996-03-07 Procede de production de solutions de polyolefines Ceased WO1996027631A1 (fr)

Priority Applications (4)

Application Number Priority Date Filing Date Title
EP96905028A EP0774481B1 (en) 1995-03-08 1996-03-07 Process for producing polyolefin solutions
CA002189868A CA2189868C (en) 1995-03-08 1996-03-07 Method of manufacturing polyolefin solutions
DE69622665T DE69622665T2 (de) 1995-03-08 1996-03-07 Verfahren zur herstellung von polyolefinlösungen
US08/737,205 US5741848A (en) 1995-03-08 1996-03-07 Method of manufacturing polyolefin solutions

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP7/77230 1995-03-08
JP7077230A JPH08245799A (ja) 1995-03-08 1995-03-08 ポリオレフィン溶液の製造方法

Publications (1)

Publication Number Publication Date
WO1996027631A1 true WO1996027631A1 (fr) 1996-09-12

Family

ID=13628066

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP1996/000564 Ceased WO1996027631A1 (fr) 1995-03-08 1996-03-07 Procede de production de solutions de polyolefines

Country Status (5)

Country Link
US (1) US5741848A (enExample)
EP (1) EP0774481B1 (enExample)
JP (1) JPH08245799A (enExample)
DE (1) DE69622665T2 (enExample)
WO (1) WO1996027631A1 (enExample)

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5861374A (en) * 1991-02-28 1999-01-19 Novo Nordisk A/S Modified Factor VII

Families Citing this family (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
ITTO20020578A1 (it) * 2002-07-03 2004-01-05 Maris Spa Flli Procedimento di produzione in continuo di una composizione comprendente gomma resina idrocarbonica e solvente
US7271209B2 (en) 2002-08-12 2007-09-18 Exxonmobil Chemical Patents Inc. Fibers and nonwovens from plasticized polyolefin compositions
US7795366B2 (en) * 2002-08-12 2010-09-14 Exxonmobil Chemical Patents Inc. Modified polyethylene compositions
US8192813B2 (en) * 2003-08-12 2012-06-05 Exxonmobil Chemical Patents, Inc. Crosslinked polyethylene articles and processes to produce same
ITTO20030764A1 (it) * 2003-10-01 2005-04-02 Maris Flli Spa Procedimento perfezionato di produzione in continuo di
EP1650251A1 (en) * 2004-10-22 2006-04-26 Teijin Twaron B.V. Method for dissolving PPTA in sulfuric acid using a twin screw extruder
US10615388B2 (en) * 2006-03-22 2020-04-07 Celgard, Llc Membrane made of a blend of UHMW polyolefins
WO2008055405A1 (en) * 2006-11-08 2008-05-15 Panpan Hu A process for producing fiber of ultra high molecular weight polyethylene
DE112011100850T5 (de) * 2010-03-08 2013-01-24 Sumitomo Chemical Co., Ltd. Ethylenpolymerpellet und Extrusionsverfahren unter Verwendung desselben

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS6189232A (ja) * 1984-09-28 1986-05-07 デーエスエム・ナムローゼ・フェンノートシャップ 高分子ポリマー均一溶液の連続製造方法
JPS61143439A (ja) * 1984-12-17 1986-07-01 Kuraray Co Ltd 高分子量ポリマ−原液の連続調製法
JPS6229447B2 (enExample) * 1979-06-19 1987-06-26 Mitsubishi Petrochemical Co
JPH08109268A (ja) * 1994-10-07 1996-04-30 Tonen Chem Corp ポリオレフィン溶液の製造方法
JPH08120093A (ja) * 1994-10-19 1996-05-14 Tonen Chem Corp ポリオレフィン溶液の製造方法

Family Cites Families (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CA957473A (en) * 1970-10-28 1974-11-12 E. I. Du Pont De Nemours And Company Process for continuously extruding crosslinkable polyethylene compositions
US3799234A (en) * 1971-02-22 1974-03-26 Welding Engineers Countercurrent vapor stripping in screw devolatilizer
US4028302A (en) * 1975-10-07 1977-06-07 E. I. Du Pont De Nemours And Company Process for preparing concentrated acrylonitrile polymer solutions
DE3577110D1 (de) * 1984-09-28 1990-05-17 Stamicarbon Verfahren zur kontinuierlichen herstellung von homogenen loesungen von hochmolekularen polymeren.
US4886279A (en) * 1988-09-15 1989-12-12 Taylor William A Circular chess/checkers board method of play

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS6229447B2 (enExample) * 1979-06-19 1987-06-26 Mitsubishi Petrochemical Co
JPS6189232A (ja) * 1984-09-28 1986-05-07 デーエスエム・ナムローゼ・フェンノートシャップ 高分子ポリマー均一溶液の連続製造方法
JPS61143439A (ja) * 1984-12-17 1986-07-01 Kuraray Co Ltd 高分子量ポリマ−原液の連続調製法
JPH08109268A (ja) * 1994-10-07 1996-04-30 Tonen Chem Corp ポリオレフィン溶液の製造方法
JPH08120093A (ja) * 1994-10-19 1996-05-14 Tonen Chem Corp ポリオレフィン溶液の製造方法

Cited By (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US5861374A (en) * 1991-02-28 1999-01-19 Novo Nordisk A/S Modified Factor VII

Also Published As

Publication number Publication date
EP0774481A4 (en) 1998-07-08
EP0774481A1 (en) 1997-05-21
JPH08245799A (ja) 1996-09-24
US5741848A (en) 1998-04-21
EP0774481B1 (en) 2002-07-31
DE69622665T2 (de) 2003-04-03
DE69622665D1 (de) 2002-09-05

Similar Documents

Publication Publication Date Title
EP1600276B1 (en) Use of a counter-rotating twin screw extruder for compounding multimodal polymer compositions
CN101511914B (zh) 聚合物配混方法
AU2005334397B2 (en) Counter-rotating twin screw extruder
US8262925B2 (en) Method for producing a phase-change material composition
CA2770973C (en) Process of producing thermoplastic starch/polymer blends
CN107814996B (zh) 一种可交联聚乙烯改性料的制备方法
JP7065952B2 (ja) 押出しポリアミド発泡体を製造するための方法
EP3464439A1 (en) Molecular modification of polyethylene resin
CN100398589C (zh) 聚合物加工用助剂和加工方法
KR100860731B1 (ko) 수지의 필름상 물질 제조방법 및 수지의 필름상 물질
EP1501892B1 (en) Improved processing of bimodal polymers
JP7638678B2 (ja) ペレット
JPH08245799A (ja) ポリオレフィン溶液の製造方法
JPH07164434A (ja) 重合α−オレフィン樹脂を配合する方法
WO2006023213A1 (en) Oxygen tailoring of polyethylene resins
US7049361B2 (en) Polyolefin series resinfilm, composition for preparing the same, process for preparing the composition for preparing the same, and apparatus for preparing the same
KR20130000331A (ko) 미세 지분 함유 수지조성물의 제조방법
JPH08109268A (ja) ポリオレフィン溶液の製造方法
JPH08245798A (ja) ポリオレフィン溶液の製造方法
EP1245619B1 (en) A polyolefin based resin film and a composition for a polyolefin type resin film
JPH08120093A (ja) ポリオレフィン溶液の製造方法
AU2006297719B8 (en) A method to increase production rate of a continuous mixer or extruder
CN109955458A (zh) 一种低挥发性树脂的制备装置及其制备方法
Lechner The Co‐rotating Twin‐Screw Extruder for Reactive Extrusion
JPH10202652A (ja) 二軸混練機による材料混練方法

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): CA US

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH DE DK ES FI FR GB GR IE IT LU MC NL PT SE

WWE Wipo information: entry into national phase

Ref document number: 2189868

Country of ref document: CA

Ref document number: 08737205

Country of ref document: US

121 Ep: the epo has been informed by wipo that ep was designated in this application
WWE Wipo information: entry into national phase

Ref document number: 1996905028

Country of ref document: EP

WWP Wipo information: published in national office

Ref document number: 1996905028

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 1996905028

Country of ref document: EP