WO1995031831A1 - Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device - Google Patents

Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device Download PDF

Info

Publication number
WO1995031831A1
WO1995031831A1 PCT/IB1995/000349 IB9500349W WO9531831A1 WO 1995031831 A1 WO1995031831 A1 WO 1995031831A1 IB 9500349 W IB9500349 W IB 9500349W WO 9531831 A1 WO9531831 A1 WO 9531831A1
Authority
WO
WIPO (PCT)
Prior art keywords
substrate
conjugated
layer
film
providing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Ceased
Application number
PCT/IB1995/000349
Other languages
English (en)
French (fr)
Inventor
Aemilianus Gradus Johannus Staring
Dirk Jan Broer
Robert Jozef Catharina Emiel Demandt
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Koninklijke Philips NV
Philips Norden AB
Original Assignee
Philips Electronics NV
Philips Norden AB
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Philips Electronics NV, Philips Norden AB filed Critical Philips Electronics NV
Priority to DE69506215T priority Critical patent/DE69506215T2/de
Priority to JP52949095A priority patent/JP3738031B2/ja
Priority to EP95916000A priority patent/EP0714557B1/en
Publication of WO1995031831A1 publication Critical patent/WO1995031831A1/en
Anticipated expiration legal-status Critical
Ceased legal-status Critical Current

Links

Classifications

    • C—CHEMISTRY; METALLURGY
    • C08—ORGANIC MACROMOLECULAR COMPOUNDS; THEIR PREPARATION OR CHEMICAL WORKING-UP; COMPOSITIONS BASED THEREON
    • C08G—MACROMOLECULAR COMPOUNDS OBTAINED OTHERWISE THAN BY REACTIONS ONLY INVOLVING UNSATURATED CARBON-TO-CARBON BONDS
    • C08G61/00—Macromolecular compounds obtained by reactions forming a carbon-to-carbon link in the main chain of the macromolecule
    • C08G61/02—Macromolecular compounds containing only carbon atoms in the main chain of the macromolecule, e.g. polyxylylenes
    • C—CHEMISTRY; METALLURGY
    • C09—DYES; PAINTS; POLISHES; NATURAL RESINS; ADHESIVES; COMPOSITIONS NOT OTHERWISE PROVIDED FOR; APPLICATIONS OF MATERIALS NOT OTHERWISE PROVIDED FOR
    • C09K—MATERIALS FOR MISCELLANEOUS APPLICATIONS, NOT PROVIDED FOR ELSEWHERE
    • C09K11/00—Luminescent materials, e.g. electroluminescent or chemiluminescent
    • C09K11/06—Luminescent materials, e.g. electroluminescent or chemiluminescent containing organic luminescent materials
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10K—ORGANIC ELECTRIC SOLID-STATE DEVICES
    • H10K50/00—Organic light-emitting devices
    • H10K50/10—OLEDs or polymer light-emitting diodes [PLED]
    • H10K50/11—OLEDs or polymer light-emitting diodes [PLED] characterised by the electroluminescent [EL] layers
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10K—ORGANIC ELECTRIC SOLID-STATE DEVICES
    • H10K50/00—Organic light-emitting devices
    • H10K50/80—Constructional details
    • H10K50/868—Arrangements for polarized light emission

Definitions

  • the invention relates to a method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (CVD).
  • CVD chemical vapour deposition
  • the invention also relates to a method of manufacturing an electroluminescent (EL) device, in particular a light-emitting diode (LED), in which use is made of such a conjugated polymer.
  • EL electroluminescent
  • LED light-emitting diode
  • Solid-state LEDs have found widespread application, for example, in displays and indicator lamps.
  • active or emissive layer in EL structures use is generally made of traditional III-V semiconductor compounds, such as doped GaAs and GaP.
  • III-V semiconductor compounds such as doped GaAs and GaP.
  • the action is based on recombinations of electron-hole pairs which are injected into the semiconductor material from electrodes situated on either side of the active layer.
  • energy is released in the form of (visible) light; this phenomenon is commonly referred to as electroluminescence.
  • the wavelength and hence the colour of the emitted light is determined by the band gap of the semiconductor material.
  • Semiconductive organic polymers expands the number of materials which can be used in EL devices.
  • Semiconductive, organic polymers have a conjugated polymeric chain.
  • the band gap, the electron affinity and the ionization potential can be adjusted by choosing the proper conjugated polymeric chains and suitable side chains.
  • such polymers enable flexible substrates to be used.
  • Conjugated polymers which can suitably be used as the active layer in EL devices are derivatives of poly(p-phenylene vinylene) (PPV), such as PPV itself and poly(2- methoxy, 5-(2'-ethylhexyloxy)-p-phenylene vinylene) (MEH-PPV).
  • PPV poly(p-phenylene vinylene)
  • MEH-PPV poly(2- methoxy, 5-(2'-ethylhexyloxy)-p-phenylene vinylene)
  • a disadvantage of spin coating is that the films formed are generally insufficiently uniform to be used in EL devices, in particular if substrates are used which are not flat.
  • the known methods are less suited for the manufacture of a polymeric layer having a predetermined thickness and uniformity.
  • the method must be continuous, without the necessity of purifying or reprocessing of the polymeric intermediate products formed, which are generally instable.
  • the invention further aims at providing a method of manufacturing a LED whose active layer is formed by a conjugated polymer of substituted or unsubstituted PPV.
  • R 1 and R 2 represent a halogen atom and R and m have the above-mentioned meaning, in a first thermal zone at a temperature of from approximately 50°C to approximately 250° C, b. transporting the evaporated monomeric compound through a second thermal zone at a temperature of from approximately 500°C to approximately 900°C, thereby forming a conjugated precursor, c. transporting the precursor of step b. to a third thermal zone in which the substrate is placed at a temperature below 500° C, thereby forming the film of the polymer of formula (I) on the substrate.
  • Suitable alkyl groups R are methyl, ethyl, propyl, butyl and pentyl groups, either branched or unbranched.
  • Suitable alkoxy groups R are methoxy, ethoxy, propoxy, butoxy and pentoxy groups, either branched or unbranched. Due to the lower vapour pressure, methyl and methoxy groups are preferred.
  • R 1 and R 2 use is preferably made of a bromine atom on account of the reactivity in the thermal elimination process.
  • a very suitable monomer is ⁇ , ⁇ '-dibromo-2-cyano-p-xylene (see formula V of Fig. 2), which can be prepared by refluxing a mixture of 2,5-dimethylbenzonitryl, N-bromosuccinimide and benzoyl peroxide in carbon tetrachloride for several hours. The solid formed is recrystallized from a mixture of petroleum ether and toluene and subsequently dried under a vacuum.
  • Another suitable monomer is o, ⁇ '-dibromo-2-methoxy-p-xylene (see formula VI of Fig.
  • the monomers evaporate in the first thermal zone at a temperature in the range between approximately 50°C and approximately 250°C, in particular between approximately 80°C and approximately 150°C. To preclude hot spots, the temperature of the monomer is preferably slowly increased to the desired value.
  • 2 moles of HC1 or HBr are split off per mole of monomer.
  • the aromatic rings of the polymer (I) can each be substituted with one to four substituents R.
  • the substituents may be different or the same.
  • the rings may comprise the same or different substituent(s).
  • the polymer is a copolymer or terpolymer.
  • a conjugated copolymer or terpolymer can be prepared by using, respectively, two or three different monomers (II). If different monomers are used, it is desirable that they all have approximately the same vapour pressure in order to obtain an optimum control of the ultimate polymeric composition. If the vapour pressures differ widely, the monomers can be evaporated in separate zones at adapted temperatures and finally be separately transported to the third thermal (substrate) zone.
  • the degree of polymerization n of the conjugated polymer (I) ranges between 10 and 100,000.
  • the film of the conjugated polymer (I) formed generally has a layer thickness in the range between 50 and 250 nm, in particular between 100 and 200 nm.
  • the growth rate of the polymeric film depends on the velocity of the carrier gas and the temperature in the first thermal zone and ranges between 100 nm and 10 ⁇ m/hour.
  • the substrate is formed by a layer of an electrode material (which will be specified hereinbelow) on, for example, a transparent, flexible foil of synthetic resin which is resistant to the prevailing temperature in the third thermal zone.
  • an electrode material which will be specified hereinbelow
  • a synthetic resin substrate preferably, polyimide or polytetrafluoroethylene is employed because of the temperature resistance.
  • the substrate is preferably provided on a substrate holder which enables the substrate to be heated or cooled to the desired temperature. In that case, the third thermal zone is formed by the substrate itself.
  • the temperature of the third thermal zone is below approximately 100°C, a non-conjugated precursor polymer is formed which can be converted to a conjugated polymer by heating to a temperature above 100°C. If the temperature of the third thermal zone is higher than approximately 100°C, a conjugated polymeric (I) film is directly formed.
  • the walls of the third thermal zone themselves may constitute the substrate on which the polymeric film is formed, or a special substrate of a specific shape can be placed inside the third thermal zone.
  • the object of providing a method of manufacturing an LED is achieved in accordance with the invention by a method which is characterized by the following steps: a. providing a first, transparent electroconductive layer on a substrate, b. providing the first layer with an active layer comprising at least one layer of a conjugated poly(p-phenylene vinylene) in accordance with formula (I) by means of a CVD process, by using a monomer in accordance with formula (II), as described above, c. providing a second electroconductive layer on the active layer.
  • the substrate use can be made of the above-mentioned inorganic substrate, but preferably use is made of transparent, flexible polymeric substrates, such as polyimide, polytetrafluoroethylene or polyethylene terephtalate.
  • transparent, flexible polymeric substrates such as polyimide, polytetrafluoroethylene or polyethylene terephtalate.
  • the polymeric substrate in one direction with a velvet cloth or to stretch it in one direction before the various layers are provided. If the conjugated polymer is deposited on such a substrate, said polymer exhibits a uniaxial orientation which is parallel to the direction of rubbing. As a result, the light emitted by an LED having such an oriented, active layer is polarized, the plane of polarization extending parallel to the direction of rubbing.
  • the substrate is provided with a first, transparent electroconductive layer which serves as the electrode for the injection of holes into the active layer of conjugated PPV to be provided on said electroconductive layer.
  • the material of this first layer has a high work function and is constituted by, for example, a thin layer of gold or silver or, preferably, by a layer of indium oxide or indium-tin oxide (ITO).
  • ITO indium oxide or indium-tin oxide
  • This first layer must be transparent to the light emitting from the active layer. In particular ITO is very suitable due to its good electrical conductivity and high transparency.
  • This first layer can be provided on the substrate by means of methods which are known per se, such as vapour deposition, sputtering or chemical vapour deposition.
  • the active layer of conjugated PPV is provided on said first electroconductive layer by means of the above-described CVD process.
  • the active layer may consist of a single layer, but may alternatively comprise more, for example three, layers of different types of conjugated PPV.
  • the layer adjoining the first electroconductive layer is then optimized for the injection of holes and comprises conjugated PPV which is substituted with electron-donating groups, such as alkoxy groups.
  • the layer adjoining the second electroconductive layer is optimized for the injection of electrons and comprises conjugated PPV which is substituted with electron-accepting groups, such as CN groups.
  • a layer of, for example, unsubstituted PPV is situated between the two boundary layers.
  • the active layer may alternatively be built up of a multilayer of two types of conjugated PPV (for example in accordance with formulas IX and X) which are alternately provided.
  • Each of said types of layers has a thickness of from 1 to 10 nm.
  • a so-called quantum well structure is formed by means of which different emission wavelengths are obtained.
  • These multilayer structures of different types of PPV can be obtained in a simple manner by means of the method in accordance with the invention, by using different types of monomers which are successively or alternately passed through the second and third thermal zone of the furnace.
  • the number of first thermal zones used in the method then corresponds to the number of different types of monomers. In that case, the first thermal zones are connected to the second thermal zones by means of valves.
  • the active layer is provided with a second electroconductive layer which serves as the electrode for the injection of electrons into the active layer.
  • the material of this layer has a low work function and consists of a layer of, for example, indium, calcium, barium or magnesium.
  • This second layer can also be provided by means of the above- mentioned methods. In particular when reactive barium is used, it is efficacious to cover said second electroconductive layer with a protective layer of, for example, epoxy or an inert metal.
  • FIG. 1 diagrammatically shows a device for the application of the method in accordance with the invention
  • Fig. 2 shows the formulas of the conjugated polymer PPV (I, IX, X and XI), of monomers (II) to (VII) which can suitably be used in the method in accordance with the invention, and of a conjugated precursor (VIII) formed by the method in accordance with the invention,
  • Fig. 3 is a diagrammatic cross-sectional view of an EL device, in particular a LED, comprising an active layer of PPV obtained by means of the method in accordance with the invention, and
  • Fig. 4 shows an I-V and L-V characteristic of an LED manufactured by means of the method in accordance with the invention.
  • Fig. 1 diagrammatically shows a device for carrying out the method in accordance with the invention.
  • a tubular furnace 1 of quartz glass is shown, in which a solid or liquid monomeric compound 2 is placed in a first thermal zone which is heated by heating elements 3.
  • the temperature ranges between approximately 50°C and 250°C.
  • a vacuum pump (not shown) which is connected to an aperture 4 is used to maintain a partial vacuum of less than 10 Pa in the furnace.
  • An aperture 10 is provided with a needle valve (not shown) having a capillary tube.
  • Arrow 5 indicates a stream of an argon carrier gas which transports the monomer 2 in the vapour state to a second thermal zone heated by heating elements 6, thereby forming a conjugated precursor (formula VIII in Fig. 2).
  • the temperature in the second thermal zone ranges between approximately 500 °C and 900° C.
  • the carrier gas and the conjugated precursor are led to a third thermal zone 7 where the temperature is below 500°C and in which zone there is a substrate 8.
  • a polymeric film 9 is formed on the substrate 8.
  • the layer 9 obtained has a very uniform layer thickness. If the temperature in zone 7 is below approximately 100°C, a non-conjugated precursor polymer is formed. If the temperature is above 100°C, conjugated PPV in accordance with formula (I) is formed.
  • the thickness can be monitored by means of a quartz crystal oscillator which is arranged in the vicinity of the substrate 8. Exemplary embodiment 2.
  • ⁇ . ⁇ f'-dibromo-p-xylene (formula IV in Fig. 2; supplier Aldrich) is placed in the position indicated by reference numeral 2 (Fig. 1).
  • the heating elements 3 are slowly heated to 150°C.
  • the second thermal zone is heated to 710°C by heating elements 6, while the third thermal zone 7 is heated to 200°C.
  • Flat, glass substrates are placed in the position indicated by reference numeral 8.
  • the entire arrangement is evacuated to a pressure of 10 ⁇ 3 Pa, whereafter a nitrogen stream is adjusted by means of the needle valve at reference numeral 10 to obtain a pressure of 0.1 Pa.
  • a transparent film 9 of conjugated PPV (formula IX of Fig. 2) having a layer thickness of 200 nm is deposited on the glass substrates 8. The film exhibits electroluminescence in the green spectral range, with maximum emission around 550 nm.
  • Exemplary embodiment 3 Exemplary embodiment 2 is repeated, with this difference that the third thermal zone 7 is not heated and the substrate is maintained at room temperature.
  • a film of a non-conjugated precursor polymer comprising one bromine atom per monomeric unit is deposited on the substrate. After heating the substrate to 220°C for 1.5 hours at a pressure of 0.1 Pa, a film of conjugated PPV (formula IX of Fig. 2) is formed which is identical to the film obtained according to exemplary embodiment 2.
  • Exemplary embodiment 1 is repeated, with this difference that ⁇ , ⁇ '- dibromo-2-cyano-p-xylene (see formula V of Fig. 2) is used as the monomer.
  • ⁇ , ⁇ '- dibromo-2-cyano-p-xylene see formula V of Fig. 2
  • this monomer is prepared in accordance with a method which is analogous to the one described by M. Hubert et. al. in J.
  • a transparent film 9 of conjugated PPV (formula X of Fig. 2) substituted with a CN group is deposited on the glass substrates 8 in a layer thickness of 200 nm.
  • the film exhibits electroluminescence in the green spectral range, with maximum emission around 540 nm.
  • Exemplary embodiment 1 is repeated, with this difference that the monomer used is ⁇ ,c-'-dibromo-2-methoxy-p-xylene (see formula VI of Fig. 2).
  • This monomer is prepared according to the method described by M. Hubert et. al. in J. Org. Chem., 45, 4496-4498 (1980), starting from 2,5-dimethylanisol (supplier Aldrich).
  • a transparent film 9 of conjugated PPV (formula XI of Fig. 2) substituted with a methoxy group is deposited on the glass substrates 8 in a layer thickness of 200 nm. The film exhibits electroluminescence in the yellow spectral range, with maximum emission around 610 nm.
  • reference numeral 1 refers to a diagrammatically represented cross-sectional view of a polymeric LED structure.
  • a transparent indium-tin oxide layer
  • ITO 5 having a surface resistance below 20 ⁇ /square is sputtered on to a glass substrate 3.
  • Said layer 5 serves as the electrode layer for injecting holes in the active layer 7 of conjugated PPV (formula IX of Fig. 2) which is to be subsequently deposited.
  • This active layer 7 has a thickness of 150 nm and is manufactured in accordance with the method described in exemplary embodiment 2.
  • a calcium layer 9 is vapour deposited on to this active layer 7 at a pressure below 2.10"* Pa.
  • the calcium layer 9 has a layer thickness of 250 nm and serves as the electrode for injecting electrons into the active layer 7.
  • the size of the polymeric LED is 1 cm 2 .
  • Both electrode layers 5 and 9 are connected to a DC source.
  • the polymeric film 7 of conjugated PPV emits homogeneous green light which is clearly visible under daylight circumstances.
  • the efficiency attained is 0.1 %, i.e. one photon is generated per 1,000 electrons injected into the active layer.
  • Fig. 4 shows the characteristic of the LED obtained, the current I, in
  • Ampere being plotted as a function of the applied voltage V, in volts, between the electrodes.
  • the quantity of light L is shown, in arbitrary units (a.u.) as a function of the voltage V.
  • the method in accordance with the invention enables polymeric LEDs having a large surface area to be manufactured in a simple manner by means of a CVD process, the active layer of said LEDs being constituted by a conjugated PPV based on readily available monomers.
  • the layer thickness of the active layer is uniform, so that the method is particularly suitable for large and/or non-planar substrates.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Organic Chemistry (AREA)
  • Polymers & Plastics (AREA)
  • Health & Medical Sciences (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • Medicinal Chemistry (AREA)
  • Physics & Mathematics (AREA)
  • Optics & Photonics (AREA)
  • Engineering & Computer Science (AREA)
  • Materials Engineering (AREA)
  • Electroluminescent Light Sources (AREA)
  • Polyoxymethylene Polymers And Polymers With Carbon-To-Carbon Bonds (AREA)
  • Manufacture Of Macromolecular Shaped Articles (AREA)
PCT/IB1995/000349 1994-05-18 1995-05-10 Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device Ceased WO1995031831A1 (en)

Priority Applications (3)

Application Number Priority Date Filing Date Title
DE69506215T DE69506215T2 (de) 1994-05-18 1995-05-10 Verfahren zur herstellung einer dünnen schicht aus konjugiertem, substituiertem oder nicht-substituiertem poly(p-phenylen-vinylen) mittels gasphasenabscheidung und herstellungsverfahren einer elektrolumineszierenden vorrichtung
JP52949095A JP3738031B2 (ja) 1994-05-18 1995-05-10 化学蒸着(CVD)による基板上への共役置換又は共役非置換ポリ(p−フェニレンビニレン)フィルムの製造方法及びエレクトロルミネセンス(EL)装置の製造方法
EP95916000A EP0714557B1 (en) 1994-05-18 1995-05-10 Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
EP94201406.9 1994-05-18
EP94201406 1994-05-18

Publications (1)

Publication Number Publication Date
WO1995031831A1 true WO1995031831A1 (en) 1995-11-23

Family

ID=8216884

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/IB1995/000349 Ceased WO1995031831A1 (en) 1994-05-18 1995-05-10 Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device

Country Status (5)

Country Link
US (1) US5670212A (enExample)
EP (1) EP0714557B1 (enExample)
JP (1) JP3738031B2 (enExample)
DE (1) DE69506215T2 (enExample)
WO (1) WO1995031831A1 (enExample)

Cited By (19)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0702505A3 (en) * 1994-09-14 1996-10-09 Mitsui Petrochemical Ind Organic electroluminescent device and method of manufacturing the same
WO1998044573A1 (en) * 1997-03-31 1998-10-08 Massachusetts Institute Of Technology Thin film fabrication
WO1999017892A1 (en) * 1997-10-03 1999-04-15 Massachusetts Institute Of Technology Selective chemical vapor deposition of polymers
WO2002096970A1 (en) * 2001-05-29 2002-12-05 Koninklijke Philips Electronics N.V. Polymer, method of its preparation, and electronic device
WO2003107450A1 (de) * 2002-06-13 2003-12-24 Siemens Aktiengesellschaft Substrat für einen organischen feld-effekt transistor, verwendung des substrates, verfahren zur erhöhung der ladungsträgermobilität und organischer feld-effekt transistor (ofet)
US7064345B2 (en) 2001-12-11 2006-06-20 Siemens Aktiengesellschaft Organic field effect transistor with off-set threshold voltage and the use thereof
US7223995B2 (en) 2002-03-21 2007-05-29 Polyic Gmbh & Co. Kg Logic components comprising organic field effect transistors
US7229868B2 (en) 2000-12-08 2007-06-12 Polyic Gmbh & Co. Kg Organic field-effect transistor, method for structuring an OFET and integrated circuit
US7238961B2 (en) 2001-02-09 2007-07-03 Polyic Gmbh & Co. Kg Organic field effect transistor with a photostructured gate dielectric, method for the production and use thereof in organic electronics
US7298023B2 (en) 2001-10-16 2007-11-20 Polyic Gmbh & Co. Kg Electronic device with organic insulator
US7329559B2 (en) 2003-01-21 2008-02-12 Polyic Gmbh & Co. Kg Use of conductive carbon black/graphite mixtures for the production of low-cost electronics
US7414513B2 (en) 2002-08-23 2008-08-19 Polyic Gmbh & Co. Kg Organic component for overvoltage protection and associated circuit
US7442954B2 (en) 2002-11-19 2008-10-28 Polyic Gmbh & Co. Kg Organic electronic component comprising a patterned, semi-conducting functional layer and a method for producing said component
US7479670B2 (en) 2003-08-25 2009-01-20 Polyic Gmbh & Co Kg Organic electronic component with high resolution structuring, and method of the production thereof
US7483275B2 (en) 2001-10-18 2009-01-27 Polyic Gmbh & Co. Kg Electronic unit, circuit design for the same, and production method
US7534034B2 (en) 2000-12-08 2009-05-19 Polyic Gmbh & Co. Kg Device for detecting at least one environmental influence
US7576294B2 (en) 2003-09-03 2009-08-18 Polyic Gmbh & Co. Kg Mechanical control elements for organic polymer electronic devices
US7589553B2 (en) 2005-03-01 2009-09-15 Polyic Gmbh & Co. Kg Electronic module with organic logic circuit elements
US7641857B2 (en) 2002-11-14 2010-01-05 Polyic Gmbh & Co. Kg Measuring apparatus used for determining an analyte in a liquid sample, comprising polymer electronic components

Families Citing this family (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
AU4048897A (en) 1996-08-12 1998-03-06 Trustees Of Princeton University, The Non-polymeric flexible organic light emitting device
US6337102B1 (en) * 1997-11-17 2002-01-08 The Trustees Of Princeton University Low pressure vapor phase deposition of organic thin films
JP3190886B2 (ja) * 1998-06-17 2001-07-23 日本電気株式会社 高分子膜の成長方法
US20040043140A1 (en) * 2002-08-21 2004-03-04 Ramesh Jagannathan Solid state lighting using compressed fluid coatings
US20040043138A1 (en) * 2002-08-21 2004-03-04 Ramesh Jagannathan Solid state lighting using compressed fluid coatings
US7611587B2 (en) * 2003-05-16 2009-11-03 Chow Peter P Thin-film deposition evaporator
US7575781B2 (en) * 2004-08-03 2009-08-18 Sur Modics, Inc. Method for depositing a polymeric coating on a substrate
KR101113920B1 (ko) * 2004-11-01 2012-02-29 에이전시 포 사이언스, 테크놀로지 앤드 리서치 폴리(아릴렌비닐렌) 및 폴리(헤테로아릴렌비닐렌) 발광폴리머 및 폴리머 발광 장치
CN113583218B (zh) * 2020-04-30 2022-11-22 中国科学院化学研究所 一种二维共轭聚合物异质结及其制备方法和应用

Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1992016023A1 (en) * 1991-02-27 1992-09-17 The Regents Of The University Of California Visible light emitting diodes fabricated from soluble semiconducting polymers

Family Cites Families (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
NL8700986A (nl) * 1987-04-27 1988-11-16 Philips Nv Poly-1,2-azepine, werkwijze voor de bereiding van een film van een dergelijk polymeer op een substraat en substraat voorzien van een dergelijk polymeer.

Patent Citations (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
WO1992016023A1 (en) * 1991-02-27 1992-09-17 The Regents Of The University Of California Visible light emitting diodes fabricated from soluble semiconducting polymers

Non-Patent Citations (2)

* Cited by examiner, † Cited by third party
Title
CHEMISTRY LETTERS, Volume, 1991, SHOUJI IWATSUKI et al., "New Method for Preparation of Poly(phenylene-vinylene) Film", page 1071 - page 1074. *
SYNTHETIC METALS, Volume 67, November 1994, E.G.J. STARING et al., "Chemical vapour deposition of poly(1,4-phenylenevinylene) films", page 71 - page 75. *

Cited By (21)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
US6143433A (en) * 1994-09-14 2000-11-07 Mitsui Chemicals, Inc. Organic electroluminescent device and process for producing the same
EP0702505A3 (en) * 1994-09-14 1996-10-09 Mitsui Petrochemical Ind Organic electroluminescent device and method of manufacturing the same
WO1998044573A1 (en) * 1997-03-31 1998-10-08 Massachusetts Institute Of Technology Thin film fabrication
WO1999017892A1 (en) * 1997-10-03 1999-04-15 Massachusetts Institute Of Technology Selective chemical vapor deposition of polymers
US7534034B2 (en) 2000-12-08 2009-05-19 Polyic Gmbh & Co. Kg Device for detecting at least one environmental influence
US7229868B2 (en) 2000-12-08 2007-06-12 Polyic Gmbh & Co. Kg Organic field-effect transistor, method for structuring an OFET and integrated circuit
US7238961B2 (en) 2001-02-09 2007-07-03 Polyic Gmbh & Co. Kg Organic field effect transistor with a photostructured gate dielectric, method for the production and use thereof in organic electronics
WO2002096970A1 (en) * 2001-05-29 2002-12-05 Koninklijke Philips Electronics N.V. Polymer, method of its preparation, and electronic device
US7298023B2 (en) 2001-10-16 2007-11-20 Polyic Gmbh & Co. Kg Electronic device with organic insulator
US7483275B2 (en) 2001-10-18 2009-01-27 Polyic Gmbh & Co. Kg Electronic unit, circuit design for the same, and production method
US7064345B2 (en) 2001-12-11 2006-06-20 Siemens Aktiengesellschaft Organic field effect transistor with off-set threshold voltage and the use thereof
US7223995B2 (en) 2002-03-21 2007-05-29 Polyic Gmbh & Co. Kg Logic components comprising organic field effect transistors
WO2003107450A1 (de) * 2002-06-13 2003-12-24 Siemens Aktiengesellschaft Substrat für einen organischen feld-effekt transistor, verwendung des substrates, verfahren zur erhöhung der ladungsträgermobilität und organischer feld-effekt transistor (ofet)
US7709865B2 (en) * 2002-06-13 2010-05-04 Polyic Gmbh & Co. Kg Substrate for an organic field effect transistor, use of said substrate, method of increasing the charge carrier mobility, and organic field effect transistor (OFET)
US7414513B2 (en) 2002-08-23 2008-08-19 Polyic Gmbh & Co. Kg Organic component for overvoltage protection and associated circuit
US7641857B2 (en) 2002-11-14 2010-01-05 Polyic Gmbh & Co. Kg Measuring apparatus used for determining an analyte in a liquid sample, comprising polymer electronic components
US7442954B2 (en) 2002-11-19 2008-10-28 Polyic Gmbh & Co. Kg Organic electronic component comprising a patterned, semi-conducting functional layer and a method for producing said component
US7329559B2 (en) 2003-01-21 2008-02-12 Polyic Gmbh & Co. Kg Use of conductive carbon black/graphite mixtures for the production of low-cost electronics
US7479670B2 (en) 2003-08-25 2009-01-20 Polyic Gmbh & Co Kg Organic electronic component with high resolution structuring, and method of the production thereof
US7576294B2 (en) 2003-09-03 2009-08-18 Polyic Gmbh & Co. Kg Mechanical control elements for organic polymer electronic devices
US7589553B2 (en) 2005-03-01 2009-09-15 Polyic Gmbh & Co. Kg Electronic module with organic logic circuit elements

Also Published As

Publication number Publication date
EP0714557A1 (en) 1996-06-05
DE69506215D1 (de) 1999-01-07
JPH09500929A (ja) 1997-01-28
US5670212A (en) 1997-09-23
EP0714557B1 (en) 1998-11-25
DE69506215T2 (de) 1999-06-10
JP3738031B2 (ja) 2006-01-25

Similar Documents

Publication Publication Date Title
EP0714557B1 (en) Method of providing a film of conjugated, substituted or unsubstituted poly(p-phenylene vinylene) on a substrate by chemical vapour deposition (cvd), as well as a method of manufacturing an electroluminescent (el) device
Baigent et al. Light-emitting diodes fabricated with conjugated polymers—recent progress
Friend et al. Electroluminescence in conjugated polymers
Moratti et al. High electron affinity polymers for LEDs
JP3239991B2 (ja) エレクトロルミネセンス装置およびその製造方法
US7687287B2 (en) Method for fabricating a polymer L.E.D.
JP3724589B2 (ja) エレクトロルミネセンス素子
Baigent et al. Conjugated polymer light‐emitting diodes on silicon substrates
Uchiyama et al. Electroluminescence from thin film of a semiconducting oligothiophene deposited in ultrahigh vacuum
Zhang et al. Yellow electroluminescent diodes utilizing poly (2, 5-bis (cholestanoxy)-1, 4-phenylene vinylene)
Chen et al. 1 micron wavelength photo-and electroluminescence from a conjugated polymer
KR20030074783A (ko) 플라스틱 기판 위의 유기 발광 다이오드
Sun et al. Green electroluminescent emission from substituted polyacetylenes
CN100436567C (zh) 蓝光发射聚合物和使用其的有机电致发光器件
Chu et al. Electroluminescence from silyl-disubstituted PPV derivative
Choi et al. Electroluminescent behaviours of polymer/organic heterostructure devices
Itabashi et al. Multi-layer polymer light-emitting diodes prepared by vapor deposition polymerization of polyazomethine thin film
Mullemwar et al. OLEDs: Emerging technology trends and designs
Baigent et al. Surface-emitting polymer light-emitting diodes
Bulović et al. Polymeric and molecular organic light emitting devices: A comparison
Vannikov et al. Electroluminscence in Ether-substituted Poly (phenylenevinylenes)
US8232116B2 (en) Method for fabricating a polymer L.E.D.
Hwang et al. White electroluminescent devices using polymer blends
Huang et al. High-brightness white light-emitting organic electroluminescent devices using poly (N-vinylcarbazole) as a hole-transporter
Dong-ge et al. Photoluminescence and Electroluminescence of the Blue Emission of Devices Based on Poly (p-Phenylenevinylene) Copolymers

Legal Events

Date Code Title Description
AK Designated states

Kind code of ref document: A1

Designated state(s): JP

AL Designated countries for regional patents

Kind code of ref document: A1

Designated state(s): AT BE CH DE DK ES FR GB GR IE IT LU MC NL PT SE

WWE Wipo information: entry into national phase

Ref document number: 1995916000

Country of ref document: EP

121 Ep: the epo has been informed by wipo that ep was designated in this application
WWP Wipo information: published in national office

Ref document number: 1995916000

Country of ref document: EP

WWG Wipo information: grant in national office

Ref document number: 1995916000

Country of ref document: EP