USRE39143E1 - Method for making a wafer-pair having sealed chambers - Google Patents
Method for making a wafer-pair having sealed chambers Download PDFInfo
- Publication number
- USRE39143E1 USRE39143E1 US10/007,288 US728801A USRE39143E US RE39143 E1 USRE39143 E1 US RE39143E1 US 728801 A US728801 A US 728801A US RE39143 E USRE39143 E US RE39143E
- Authority
- US
- United States
- Prior art keywords
- wafer
- layer
- chamber
- pump
- silicon
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Lifetime
Abstract
A method for fabricating a wafer-pair having at least one recess in one wafer and the recess formed into a chamber with the attaching of the other wafer which has a port plugged with a deposited layer on its external surface. The deposition of the layer may be performed in a very low pressure environment, thus assuring the same kind of environment in the sealed chamber. The chamber may enclose at least one device such as a thermoelectric sensor, bolometer, emitter or other kind of device. The wafer-pair typically will have numerous chambers, with devices, respectively, and may be divided into a multiplicity of chips.
Description
The Government may have rights in this invention pursuant to Contract No. MDA972-95-3-002 awarded by the DARPA.
The present invention pertains to vacuum encapsulated microstructure devices. It particularly pertains to the vacuum seal of a cavity between two wafers, and more particularly to the fabrication of such two wafers having a plugable hole for evacuation of gases from the cavity.
Various devices, such as microstructure infrared (IR) devices, require vacuum encapsulation for optimal performance. Conventional vacuum packaging is complex and costly. Known prior art approaches to wafer level vacuum sealing cannot yield adequately low pressures, the best in the range of 0.5 torr. Such pressures resulted in 50 percent signal losses for thermoelectric (TE) devices as an example.
The present invention involves the sealing of two wafers together resulting in a cavity between the wafers with a plugable hole for the evacuating of gases from the cavity. The hole, after evacuation of gases from the cavity, is plugged with deposited metal. The result is an integral vacuum package (IVP). This approach permits the sealing of the two wafers together without having to create the vacuum seal at the same time. The final vacuum seal can be done in a high vacuum by either evaporation or the sputtering of a thick layer of metal to plug the small pump-out port. This approach allows a thorough baking out of the wafer to wafer seals and interior surfaces prior to a final vacuum seal. It separates the two functions and does not limit the bake-out to the solder processing steps. There is independent control over sealing and bake-out to maximize bond yield and minimize residual pressure. This approach also permits clear access of each vacuum cavity directly, thereby avoiding the need to pump from the periphery of the wafer inwards. The procedure here has been implemented and resulted in vacuum levels below 10 millitorr of residual pressure as measured by pressure sensors within the cavity. The seals cover significant substrate topography. Seals over topography of 0.25 microns have been demonstrated. The required processing temperatures are below 300 degrees Centigrade (C.). These chips can be handled with conventional chip handling equipment. Yields for this process exceed 90 percent. Costs of the present vacuum-sealed chips are 80 to 90 percent less than that of conventionally vacuum-sealed chips. The present approach results in sealed devices that have high temperature longevity for pressures below 100 millitorr; ten years is indicated by test data for ambient temperatures up to 150 degrees C. Each cavity may have a gas instead of a vacuum. Each cavity, chamber or volume may contain detectors such as thermoelectric detectors, devices, bolometers, or may contain emitters.
A process for developing chip 10 is shown in FIGS. 4a through 4m . The process for detector wafer 13 starts out with a double polished silicon wafer 13. In FIG. 4a , one micron layers 22a and 23a of thermal SiO2 are grown on wafer 13, and 0.3 micron layers 22b and 23b of low pressure chemical vapor deposited (LPCVD) Si3N4. Si3N4 layer 22b and SiO2 layer 22a are removed from the “front” of wafer 13. A 1000 angstroms of a thermal SiO2 layer 24 is grown on the front of wafer 13 in FIG. 4b. A layer 25 of 2000 angstroms of Si3N4 (bottom bridge nitride) is deposited on layer 24 in FIG. 4c. The first metal NiFe (60:40) of a thermocouple is deposited as a 1100 angstrom layer 26 on layer 25 and then first metal layer 26 is patterned with a first mask by ion milling resulting in the layout of FIG. 4d.
For the second metal of the thermocouple detectors, a thousand angstrom layer 27 of chromium is deposited on layers 25 and 26. Layer 27 in FIG. 4e is patterned with a second mask by ion milling and wet etching. A layer 28 consisting of 6000 angstroms of Si3N4 is deposited on metal layers 26 and 27, and layer 25, as the top bridge nitride in FIG. 4f. An absorber 29 is deposited on layer 28 of FIG. 4g and patterned with a third mask. Absorber 29 is capped with a layer 30 of Si3N4. Plasma etched vias 31 to metal layer 27 are patterned and cut with the use of a fourth mask, as shown in FIG. 4h. Plasma etched vias 32 in FIG. 4i for the final etch are patterned and cut with the use of a fifth mask. Five hundred angstroms of Cr, 2000 angstroms of Ni and 5000 angstroms of Au are deposited, patterned and lifted off for pad and solder frame metal 33 in FIG. 4j. Passivated leadouts 40 in first metal 26 or second metal 27 pass under the seal ring metal 33 in FIG. 4j. Plasma etched pump-out port vias 11 are patterned and cut on layers 23b and 23a of the back of wafer 13 in FIG. 4k. There is a KOH etch of the back side of wafer 13 through 90 percent of wafer 13 for port 11 in FIG. 4 l. Port 11 is completed with an etch through via 32 to the front of wafer 13 as shown in FIG. 4m.
Bonding and sealing detector wafer 13 and top cap wafer 14 are done with clean surfaces. Bonding surfaces of wafers 13 and 14 are sputter cleaned just prior to doing the wafer bond. The following sequence of events indicate how to align, bond and seal the wafer pair 13 and 14 of FIGS. 6a , 6b and 6c. To begin, the Au solder ring surface 33 of detector wafer 13 is sputter cleaned. The InPb surface of ring 18 of top cap wafer 14 is oxygen plasma cleaned. Wafers 13 and 14 of FIG. 6a are aligned in a bonding cassette using 0.002 inch spacers between the wafers. The aligned wafer pair is put in a vacuum press which is pumped to a good vacuum with a turbo pump. Wafers 13 and 14 are pressed together in FIG. 6b , with about 400 pounds of pressure. The temperature of the wafers is ramped up to 300 degrees C., which takes about one hour. Then wafers 13 and 14 are held at this achieved temperature and pressure for five minutes. Then wafers 13 and 14 are cooled down to room temperature, and the vacuum chamber is vented.
Further variations on this theme include top cap wafer 14 composed of Germanium for better IR transmission or ZnSe for broadband transmission (i.e., visible and IR) or other optical window materials for application specific optical bandpass behavior. Top cap wafer 14 may have integrated components built in or on the surface in addition to those on the detector wafer 13. Detector wafer 13 having a diaphragm pressure sensor integrated into it, the sealed chamber then forms a vacuum pressure reference. Detector wafer 13 may have infrared bolometer arrays with readout electronics integrated into the wafer. Detector wafer 13 may have moving parts to be sealed in a chamber for other functional purposes. The bonded wafer pair 13 and 14 in FIG. 6c may be hermetically sealed with a controlled residual pressure of a specific gas type for optimal thermal, mechanical or other properties rather than simply evacuated for the devices within the chamber.
Claims (66)
1. A method for making a wafer-pair having deposited layer plugged sealed chambers, comprising:
growing a thermal layer on a first side of a first silicon wafer;
depositing a nitride layer on the thermal layer;
depositing, patterning and removing portions of first metal layer on the nitride layer for a plurality of devices;
depositing, patterning and removing portions of a second metal layer on the nitride and first metal layers for the plurality of devices;
patterning and removing material from the first silicon wafer and layers on the first side of the first silicon wafer and from a second side of the first silicon wafer to make a plurality of pump-out ports through the first silicon wafer and layers on the first silicon wafer;
masking and removing material from a first side of a second silicon wafer to form a plurality of recesses in the first side of the second silicon wafer;
forming a sealing ring on the first side of the second silicon wafer around each of the plurality of recesses; and
positioning the first side of the first silicon wafer next to the first side of the second silicon wafer; and
wherein:
each sealing ring is in contact with at least one of the layers on the first side of the first silicon wafer;
each recess of the plurality of recesses results in a chamber containing at least one device of the plurality of devices;
each sealing ring encloses at least one pump-out port of the plurality of pump-out ports; and
the first and second silicon wafers are effectively a bonded together set of wafers.
2. The method of claim 1 , further comprising:
placing the set of wafers in an environment of a vacuum wherein a vacuum occurs in each chamber via the at least one pump-out port; and
depositing a layer of material on the second side of the first silicon wafer and the plurality of pump-out ports on the second side of the first silicon wafer, wherein each chamber is sealed from the environment.
3. The method of claim 2 , further comprising baking out the set of wafers prior to depositing the layer of material on the second side of the first wafer and the plurality of pump-out ports on the second side of the first silicon wafer.
4. The method of claim 3 , further comprising coating the second wafer with antireflection material.
5. The method of claim 4 , wherein the second silicon wafer is made from low oxygen silicon or float zone silicon to minimize an absorption peak in an 8-14 micron wavelength region of light going through the second silicon wafer to the plurality of devices.
6. The method of claim 5 , wherein the set of wafers is cut into a plurality of chips wherein each chip has one or more sealed chambers.
7. The method of claim 6 , wherein the plurality of devices comprise thermoelectric detectors.
8. The method of claim 6 , wherein the plurality of devices comprise bolometers.
9. A method for making a wafer-pair having at least one deposited layer plugged sealed chamber, comprising:
growing a first thermal layer on a first side of a first silicon wafer;
depositing a nitride layer on the first thermal layer;
depositing and patterning a first metal layer on the nitride layer for at least one device;
depositing and patterning a second metal layer on the nitride layer and the first metal layer for the at least one device;
patterning and removing material from the first silicon wafer and layers on the first side of the first silicon wafer and from a second side of the first silicon wafer to make a pump-out port through a first silicon wafer and the layers on the first silicon wafer;
masking and removing material from a first side of a second silicon wafer, to form a recess in the first side of the second silicon wafer;
forming a sealing ring on the first side of the second silicon wafer around the recess; and
positioning the first side of the first silicon wafer next to the first side of the second silicon wafer; and
wherein:
the sealing ring is in contact with at least one of the layers on the first side of the first silicon layer;
the at least one device is within the recess resulting in a chamber containing the at least one device;
the pump-out port is within the sealing ring; and
the first and second silicon wafers are effectively a bonded together set of wafers.
10. The method of claim 9 , further comprising:
placing the bonded together set of wafers in an environment of a vacuum wherein a vacuum occurs in the chamber via the pump-out port; and
depositing a layer of material on the second side of the first silicon wafer and the pump-out port on the second side of the first silicon wafer, wherein the chamber is sealed from the environment.
11. The method of claim 10 , further comprising baking out the bonded together set of wafers prior to depositing the layer of material on the second side of the first wafer and the pump-out port on the second side of the first silicon wafer.
12. The method of claim 11 , wherein the at least one device is a detector.
13. The method of claim 12 , further comprising coating the second silicon wafer with antireflection material.
14. The method of claim 11 , wherein the second silicon wafer is made from low oxygen silicon or float zone silicon to minimize an absorption peak in an 8-14 micron wavelength region of light going through the second silicon wafer to the at least one device.
15. The method of claim 14 , wherein the at least one device is a thermoelectric detector.
16. The method of claim 14 , wherein the at least one device is a bolometer.
17. The method of claim 11 , wherein the at least one device is an emitter.
18. A method for making a wafer-pair having at least one deposited layer plugged sealed chamber, comprising:
growing a first layer of thermal SiO2 on a first of a first silicon wafer;
depositing a first layer of Si3N4 on the first layer of thermal SiO2;
growing a second layer of thermal SiO2 on a second side of the first silicon wafer;
depositing a second layer of Si3N4 on the second layer of thermal SiO2;
depositing a layer of a first metal on the second layer of Si3N4;
patterning the layer of the first metal;
depositing a layer of a second metal on the layer of the first metal;
patterning the layer of the second metal;
depositing a third layer of Si3N4 on the layers of the first and second metals;
etching at least one via through the third layer of Si3N4, the layers of the second and first metals, the second layer of Si3N4 and the second layer of thermal SiO2;
etching a pump-out port through the first layer of SiO2 and a first portion of the silicon wafer proximate to the at least one via;
etching within the at least one via through a second portion of the silicon wafer to the pump-out port;
growing a third layer of thermal SiO2 on a first side of a second silicon wafer and a fourth layer of
thermal SiO2 on a second side of the second silicon wafer;
growing a fourth layer of Si3N4 on the third layer of thermal SiO2 and a fifth layer of Si3N4 on the fourth layer of SiO2;
patterning and cutting the fourth layer Si3N4 and the third layer of thermal SiO2 for a bond pad area;
etching a first portion of the second silicon wafer through the fourth Si3N4 layer and third SiO2 layer for the bond pad area;
patterning and cutting the fifth layer of Si3N4 and fourth layer of thermal SiO2 for a recess area;
etching a second portion from the second side of the second silicon wafer to form a recess;
applying an optical coating to the second silicon wafer to substantially reduce reflections;
applying a solder ring proximate to a perimeter of the recess, on the second side of the second silicon wafer;
aligning the first silicon wafer with the second silicon wafer, having the first side of the first silicon wafer and the second side of the second silicon wafer face each other;
putting the first and second silicon wafers in a vacuum;
pressing the first and second silicon wafers together with a pressure;
ramping the temperature of the silicon wafers up to a high temperature;
increasing the pressure of the first and second silicon wafers against each other to bond the silicon wafers to each other;
baking out the first and second silicon wafers;
cooling down the first and second silicon wafers under a maintained vacuum;
depositing a layer of a metal on the second side of the second silicon wafer to plug the pump-out port to seal the recess with a vacuum; and
removing the bonded first and second silicon wafers from the vacuum.
19. A method for making a wafer-pair having deposited layer plugged sealed chambers, comprising:
growing a thermal layer on a first side of a first silicon wafer;
patterning and removing material from the first silicon wafer and layers on the first side of the first silicon wafer and from a second side of the first silicon wafer to make a plurality of pump-out ports through the first silicon wafer and layers on the first silicon wafer;
masking and removing material from a first side of a second silicon wafer to form a plurality of recesses in the first side of the second silicon wafer;
forming a sealing ring on the first side of the second silicon wafer around each of the plurality of recesses; and
positioning the first side of the first silicon wafer next to the first side of the second silicon wafer; and
wherein:
each sealing ring is in contact with at least one of the layers on the first side of the first silicon layer;
each recess of the plurality of recesses results in a chamber;
each sealing ring encloses at least one pump-out port of the plurality of pump-out ports; and
the first and second silicon wafers are effectively a bonded together set of wafers.
20. The method of claim 19 , further comprising:
placing the set of wafers in an environment of a vacuum wherein a vacuum occurs in each chamber via a pump-out port; and
depositing a layer of material on the second side of the first silicon wafer and the plurality of pump-out out ports on the second side of the first silicon wafer, wherein each chamber is sealed from the environment.
21. The method of claim 20 , further comprising baking out the set of wafers prior to depositing the layer of material on the second side of the first wafer and the plurality of pump-out ports on the second side of the first silicon wafer.
22. The method of claim 21 , wherein the set of wafers is cut into a plurality of chips wherein each chip has one or more sealed chambers.
23. The method of claim 22 , wherein the one or more sealed chambers contains one or more devices.
24. The method of claim 19 , further comprising:
placing the set of wafers in an environment of a gas wherein the gas enters each chamber via a pump-out port; and
depositing a layer of material on the second side of the first silicon wafer and the plurality of pump-out ports on the second side of the first silicon wafer, wherein each chamber is sealed from an ambient environment.
25. A method for making a wafer-pair having deposited layer plugged sealed chambers, comprising:
growing a thermal layer on a first side of a first wafer;
depositing a nitride layer on the thermal layer;
depositing, patterning and removing portions of first metal layer on the nitride layer for a plurality of devices;
depositing, patterning and removing portions of a second metal layer on the nitride and first metal layers for the plurality of devices;
patterning and removing material from the first wafer and layers on the first side of the first wafer and from a second side of the first wafer to make a plurality of pump-out ports through the first wafer and layers on the first wafer;
masking and removing material from a first side of a second wafer to form a plurality of recesses in the first side of the second wafer;
forming a sealing ring on the first side of the second wafer around each of the plurality of recesses; and
positioning the first side of the first wafer next to the first side of the second wafer; and wherein:
each sealing ring is in contact with at least one of the layers on the first side of the first wafer;
each recess of the plurality of recesses results in a chamber containing at least one device of the plurality of devices;
each sealing ring encloses at least one pump-out port of the plurality of pump-out ports; and
the first and second wafers are effectively a bonded together set of wafers.
26. The method of claim 25 , further comprising:
placing the set of wafers in an environment of a vacuum wherein a vacuum occurs in each chamber via the at least one pump-out port; and
depositing a layer of material on the second side of the first wafer and the plurality of pump-out ports on the second side of the first wafer, wherein each chamber is sealed from the environment.
27. The method of claim 26 , further comprising baking out the set of wafers prior to depositing the layer of material on the second side of the first wafer and the plurality of pump-out ports on the second side of the first wafer.
28. The method of claim 27 , further comprising coating the second wafer with antireflection material.
29. The method of claim 28 , wherein the second wafer is made from a material that is at least substantially transparent to light in the infrared spectrum.
30. The method of claim 29 , wherein the plurality of devices comprise thermoelectric detectors.
31. The method of claim 30 , wherein the plurality of devices comprise bolometers.
32. A method for making a wafer-pair having at least one deposited layer plugged sealed chamber, comprising:
growing a first thermal layer on a first side of a first wafer;
depositing a nitride layer on the first thermal layer;
depositing and patterning a first metal layer on the nitride layer for at least one device;
depositing and patterning a second metal layer on the nitride layer and the first metal layer for the at least one device;
patterning and removing material from the first wafer and layers on the first side of the first wafer and from a second side of the first wafer to make a pump-out port through the first wafer and the layers on the first wafer;
masking and removing material from a first side of a second wafer, to form a recess in the first side of the second wafer;
forming a sealing ring on the first side of the second wafer around the recess;
positioning the first side of the first wafer next to the first side of the second wafer; and
wherein:
the sealing ring is in contact with at least one of the layers on the first side of the first wafer;
the at least one device is within the recess resulting in a chamber containing the at least one device;
the pump-out port is within the sealing ring; and
the first and second wafers are effectively a bonded together set of wafers.
33. The method of claim 32 , further comprising:
placing the bonded together set of wafers in an environment of a vacuum wherein a vacuum occurs in the chamber via the pump-out port; and
depositing a layer of material on the second side of the first wafer and the pump-out port on the second side of the first wafer, wherein the chamber is sealed from the environment.
34. The method of claim 33 , further comprising baking out the bonded together set of wafers prior to depositing the layer of material on the second side of the first wafer and the pump-out port on the second side of the first wafer.
35. The method of claim 34 , wherein the at least one device is a detector.
36. The method of claim 35 , wherein the at least one device is a thermoelectric detector.
37. The method of claim 34 , wherein the at least one device is an emitter.
38. A method for making a wafer-pair having sealed chambers, comprising:
patterning and removing material from a first wafer to make a plurality of pump-out ports through the first wafer;
masking and removing material from a first side of a second wafer to form a plurality of recesses in the first side of the second wafer;
forming a sealing ring on a first side of the first wafer or the first side of the second wafer such that the sealing ring extends around each of the plurality of recesses; and
positioning the first side of the first wafer next to the first side of the second wafer; and
wherein:
each sealing ring is in contact with the first side of the first wafer and the first side of the second wafer
each recess of the plurality of recesses results in a chamber;
each sealing ring encloses at least one pump-out port of the plurality of pump-out ports; and
the first and second wafers are effectively a bonded together set of wafers.
39. The method of claim 38 , further comprising:
placing the set of wafers in an environment of a vacuum wherein a vacuum occurs in each chamber via a pump-out port; and
depositing a layer of material on a second side of the first wafer to seal the plurality of pump-out out ports from the second side of the first wafer, wherein each chamber is sealed from the environment.
40. The method of claim 39 , further comprising baking out the set of wafers prior to depositing the layer of material on the second side of the first wafer.
41. The method of claim 40 , wherein the set of wafers is cut into a plurality of chips wherein each chip has one or more sealed chambers.
42. The method of claim 40 , wherein the one or more sealed chambers contains one or more devices.
43. The method of claim 38 , further comprising:
placing the set of wafers in an environment of a gas wherein the gas enters each chamber via a pump-out port; and
depositing a layer of material on a second side of the first wafer to seal the plurality of pump-out out ports from the second side of the first wafer, wherein each chamber is sealed from an ambient environment.
44. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer and a second wafer;
forming one or more pump-out ports through the first wafer;
positioning a first side of the first wafer next to a first side of the second wafer, the first wafer and the second wafer forming at least part of a chamber, with the pump-out port of the first wafer in fluid communication with the chamber; and
exposing the chamber to a negative pressure relative to atmosphere while plugging the pump out port to seal the chamber.
45. A method according to claim 44 further comprising the step of:
making a recess in the first side of the first wafer and/or the first side of the second wafer, wherein the recess forms part of the chamber.
46. A method according to claim 44 further comprising the step of:
providing one or more devices in or on the first side of the first wafer and/or the first side of the second wafer before the positioning step.
47. A method according to claim 46 wherein the one or more devices are in the chamber.
48. A method according to claim 46 wherein the one or more devices include an array of infrared detectors.
49. A method according to claim 44 wherein a sealing ring is positioned between the first side of the first wafer and the first side of the second wafer, and wherein the first wafer, the second wafer and the sealing ring form the chamber.
50. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer and a second wafer;
forming one or more pump-out ports through the first wafer;
making a recess in a first side of the first wafer and/or a first side of the second wafer;
positioning the first side of the first wafer next to the first side of the second wafer, the first wafer and the second wafer forming a chamber that is at least partially defined by the recess, with the pump-out port of the first wafer in fluid communication with the chamber; and
exposing the chamber to a negative pressure relative to atmosphere while plugging the pump out port to seal the chamber.
51. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer having a first side, with one or more bond pads on the first side;
providing a second wafer;
forming one or more bond-pad holes through the second wafer;
positioning the first side of the first wafer next to a first side of the second wafer; the first wafer and the second wafer forming at least part of a chamber, the first wafer and second wafer being aligned so that the bond-pad holes in the second wafer provide physical access to the one or more bond pads on the first wafer through at least selected bond-pad holes in the second wafer; and
the first and second wafers are effectively a bonded together set of wafers.
52. A bonded wafer pair, comprising:
a first wafer;
a second wafer;
the first wafer having one or more pump-out ports through the first wafer;
the first side of the first wafer bonded to a first side of the second wafer via a sealing ring; the first wafer, the second wafer and the sealing ring forming a chamber, with the pump-out port of the first wafer in fluid communication with the chamber, the chamber having a negative pressure therein relative to atmosphere; and
a plug for plugging the pump out port.
53. A bonded wafer pair according to claim 52 further comprising a recess in the first side of the first wafer and/or the first side of the second wafer, wherein the recess forms at least part of the chamber.
54. A bonded wafer pair according to claim 52 further comprising one or more devices in or on the first side of the first wafer and/or the first side of the second wafer.
55. A bonded wafer pair according to claim 54 wherein the one or more devices are in the chamber.
56. A bonded wafer pair according to claim 54 wherein the one or more devices include an array of infrared detectors.
57. A bonded wafer pair having a sealed chamber, comprising:
a first wafer;
a second wafer bonded to the first wafer;
one or more pump-out ports through the first wafer;
a recess in a first side of the first wafer and/or a first side of the second wafer;
the first wafer and the second wafer forming a chamber that includes the recess, with the pump-out port of the first wafer in fluid communication with the chamber, the chamber having a negative pressure therein relative to atmosphere; and
one or more plugs for plugging the one or more pump out ports to seal the chamber.
58. A bonded wafer pair, comprising:
a first wafer having a first side, with one or more bond pads on the first side;
a second wafer, with one or more bond-pad holes through the second wafer;
the first side of the first wafer bonded to a first side of the second wafer with a sealing ring therebetween, the first wafer and second wafer being aligned so that the bond-pad holes in the second wafer provide physical access to the one or more bond pads on the first wafer through at least selected bond-pad holes in the second wafer; and
the first wafer, the second wafer and the sealing ring forming a chamber.
59. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer and a second wafer, the first wafer having a first side and a second side;
forming one or more pump-out ports through the first wafer;
positioning the first side of the first wafer next to a first side of the second wafer, the first wafer and the second wafer forming at least part of a chamber, with the pump-out port of the first wafer in fluid communication with the chamber; and
providing one or more layer(s) in a negative pressure relative to atmosphere to a second side of the first wafer, wherein the one or more layer(s) plug the pump out port and seal the chamber.
60. A method according to claim 59 wherein the one or more layer(s) are deposited by evaporation.
61. A method according to claim 59 wherein the one or more layer(s) are deposited by sputtering.
62. A method according to claim 59 wherein the one or more layer(s) include a metal layer.
63. A method according to claim 59 wherein the one or more layer(s) are deposited in a high vacuum environment.
64. An apparatus having a sealed chamber with one or more devices positioned in the sealed chamber, the one or more devices having a desired operating temperature range, the bonded wafer pair comprising:
a first wafer;
a second wafer secured relative to the first wafer;
the first wafer and the second wafer forming a chamber that has a volume, wherein the one or more devices are positioned in the chamber;
one or more pump-out ports through the first wafer, at least one of the one or more pump-out ports in fluid communication with the chamber;
one or more plugs for plugging the one or more pump out ports to seal the chamber; and
the volume of the chamber remaining relatively constant over the desired operating temperature range of the one or more devices.
65. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer and a second wafer, the first wafer having a first side and a second side;
forming one or more pump-out ports through the first wafer;
positioning the first side of the first wafer next to a first side of the second wafer, the first wafer and the second wafer forming at least part of a chamber, with the pump-out port of the first wafer in fluid communication with the chamber; and
providing one or more layer(s) by deposition to a second side of the first wafer, wherein the one or more deposited layer(s) plug the pump out port and seal the chamber, and wherein the one or more layer(s) are deposited by evaporation.
66. A method for making a wafer-pair with a sealed chamber therebetween, comprising:
providing a first wafer and a second wafer, the first wafer having a first side and a second side;
forming one or more pump-out ports through the first wafer;
positioning the first side of the first wafer next to a first side of the second wafer, the first wafer and the second wafer forming at least part of a chamber, with the pump-out port of the first wafer in fluid communication with the chamber; and
providing one or more layer(s) by deposition to a second side of the first wafer, wherein the one or more deposited layer(s) plug the pump out port and seal the chamber, and wherein the one or more layer(s) are deposited by sputtering.