TWI834852B - Adhesive for semiconductors, manufacturing method of semiconductor device, and semiconductor device - Google Patents

Adhesive for semiconductors, manufacturing method of semiconductor device, and semiconductor device Download PDF

Info

Publication number
TWI834852B
TWI834852B TW109110054A TW109110054A TWI834852B TW I834852 B TWI834852 B TW I834852B TW 109110054 A TW109110054 A TW 109110054A TW 109110054 A TW109110054 A TW 109110054A TW I834852 B TWI834852 B TW I834852B
Authority
TW
Taiwan
Prior art keywords
adhesive
semiconductor
mass
semiconductor device
semiconductors
Prior art date
Application number
TW109110054A
Other languages
Chinese (zh)
Other versions
TW202039760A (en
Inventor
茶花幸一
秋吉利泰
林出明子
佐藤慎
Original Assignee
日商力森諾科股份有限公司
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by 日商力森諾科股份有限公司 filed Critical 日商力森諾科股份有限公司
Publication of TW202039760A publication Critical patent/TW202039760A/en
Application granted granted Critical
Publication of TWI834852B publication Critical patent/TWI834852B/en

Abstract

一種半導體用接著劑,含有重量平均分子量小於10000的樹脂、硬化劑、無機填料及矽酮橡膠填料。An adhesive for semiconductors, containing a resin with a weight average molecular weight of less than 10,000, a hardener, an inorganic filler and a silicone rubber filler.

Description

半導體用接著劑、半導體裝置的製造方法及半導體裝置Adhesive for semiconductors, manufacturing method of semiconductor device, and semiconductor device

本揭示是有關於一種半導體用接著劑、半導體裝置的製造方法及半導體裝置。The present disclosure relates to an adhesive for semiconductors, a manufacturing method of a semiconductor device, and a semiconductor device.

先前,於將半導體晶片(chip)與基板連接時,一直廣泛地應用使用金線等金屬細線的打線接合(wire bonding)方式。另一方面,為了對應針對半導體裝置的高功能化、高積體化、高速化等要求,於半導體晶片或基板上形成稱為凸塊(bump)的導電性突起而將半導體晶片與基板直接連接的覆晶連接方式(FC(flip chip)連接方式)正在推廣。Previously, when connecting a semiconductor chip (chip) to a substrate, wire bonding using thin metal wires such as gold wires has been widely used. On the other hand, in order to meet the requirements for higher functionality, higher integration, and higher speed of semiconductor devices, conductive protrusions called bumps are formed on a semiconductor wafer or a substrate to directly connect the semiconductor wafer and the substrate. The flip-chip connection method (FC (flip chip) connection method) is being promoted.

作為FC連接方式,已知有使用焊料、錫、金、銀、銅等使連接部金屬接合的方法、施加超音波振動使連接部金屬接合的方法、利用樹脂的收縮力保持機械接觸的方法等。就連接部的可靠性的觀點而言,通常為使用焊料、錫、金、銀、銅等使連接部金屬接合的方法。Known FC connection methods include a method of metal-joining the connection parts using solder, tin, gold, silver, copper, etc., a method of metal-joining the connection parts by applying ultrasonic vibration, a method of maintaining mechanical contact using the shrinkage force of resin, etc. . From the viewpoint of the reliability of the connection part, a method of metal-joining the connection part using solder, tin, gold, silver, copper, etc. is usually used.

例如,關於半導體晶片及基板間的連接,球形柵格陣列(Ball Grid Array,BGA)、晶片尺寸封裝(Chip Size Package,CSP)等中盛行使用的板上晶片(Chip On Board,COB)型連接方式亦相當於FC連接方式。另外,FC連接方式亦廣泛用於在半導體晶片上形成連接部(凸塊或配線)而將半導體晶片間連接的堆疊晶片(Chip On Chip,COC)型的連接方式(例如,參照專利文獻1)。For example, regarding the connection between semiconductor chips and substrates, Chip On Board (COB) type connections are popularly used in Ball Grid Array (BGA), Chip Size Package (CSP), etc. The method is also equivalent to the FC connection method. In addition, the FC connection method is also widely used in a Chip On Chip (COC) type connection method that forms connection portions (bumps or wiring) on semiconductor wafers to connect semiconductor wafers (for example, see Patent Document 1) .

另外,於強烈要求進一步的小型化、薄型化、高功能化的封裝中,將所述連接方式進行積層-多段化的晶片堆疊(chip stack)型封裝、封裝堆疊封裝(Package On Package,POP)、矽通孔(Through-Silicon Via,TSV)等亦開始廣泛普及。此種積層-多段化技術對半導體晶片等進行三維配置,因此與二維地配置的方法相比可縮小封裝。另外,所述積層-多段化技術於半導體的性能提高、雜訊減少、安裝面積的削減、省電力化方面亦有效,因此作為下一代的半導體配線技術而受到矚目。In addition, in packages that are strongly required to be further miniaturized, thinned, and highly functional, chip stack-type packages and package-on-package (POP) packages in which the connection method is multi-layered are being developed. , Through-Silicon Via (TSV), etc. have also begun to become widely popular. This layering-multi-segmentation technology arranges semiconductor wafers and the like in three dimensions, so the package can be reduced compared to the method of two-dimensional arrangement. In addition, the lamination-multi-segmentation technology is also effective in improving semiconductor performance, reducing noise, reducing mounting area, and saving power, and is therefore attracting attention as a next-generation semiconductor wiring technology.

另外,就提高生產性的觀點而言,於半導體晶圓上壓接(連接)半導體晶片之後單片化而製作半導體封裝的晶片堆疊晶圓(Chip On Wafer,COW)、於半導體晶圓彼此壓接(連接)之後單片化而製作半導體封裝的晶圓堆疊晶圓(Wafer On Wafer,WOW)亦受到矚目。進而,就同樣的觀點而言,於將多個半導體晶片對位並暫時壓接在半導體晶圓上或鑄模陣列封裝(Mold Array Package,MAP)基板上之後,一併正式壓接該些多個半導體晶片來確保連接的多端子接合(Gang bonding)方式亦受到矚目。 [現有技術文獻] [專利文獻]In addition, from the viewpoint of improving productivity, a chip on wafer (COW) in which semiconductor wafers are pressed (connected) onto a semiconductor wafer and then singulated to produce a semiconductor package, the semiconductor wafers are pressed against each other. Wafer on wafer (WOW), which is connected (connected) and then monolithized to produce semiconductor packages, is also attracting attention. Furthermore, from the same point of view, after a plurality of semiconductor wafers are aligned and temporarily press-bonded on the semiconductor wafer or a mold array package (Mold Array Package, MAP) substrate, the plurality of semiconductor wafers are formally press-bonded together. The multi-terminal bonding (Gang bonding) method of using semiconductor chips to ensure connections is also attracting attention. [Prior Art Document] [Patent Document]

專利文獻1:日本專利特開2008-294382號公報Patent Document 1: Japanese Patent Application Publication No. 2008-294382

[發明所欲解決之課題] 在覆晶封裝中,有時由於半導體用接著劑與半導體晶片之間以及半導體晶片與基板之間的熱膨脹係數的差而產生應力,並在封裝中產生翹曲。隨著半導體晶片及半導體晶圓的薄膜化,更容易發生所述封裝的翹曲。[Problem to be solved by the invention] In flip-chip packages, stress may occur due to differences in thermal expansion coefficients between the semiconductor adhesive and the semiconductor wafer and between the semiconductor wafer and the substrate, causing warpage in the package. As semiconductor chips and semiconductor wafers become thinner, warpage of the package becomes more likely to occur.

另外,在所述積層-多段化的晶片堆疊型封裝中,與一段的晶片堆疊型封裝相比,翹曲容易變大。In addition, in the multi-layered wafer stacked package, the warpage is likely to be greater compared to the one-stage wafer stacked package.

由於所述封裝的翹曲,容易發生無法進行二次成型(overmold)以及發生封裝的連接不良的問題。因此,強烈要求封裝的低翹曲化。Due to the warpage of the package, problems such as overmold failure and poor connection of the package easily occur. Therefore, there is a strong demand for low package warpage.

此處,作為實現封裝的低翹曲化的方法,考慮到使半導體用接著劑低彈性化。作為使半導體用接著劑低彈性化的方法,考慮到使高分子成分的玻璃轉移溫度低溫化的方法、減少無機填料的添加量的方法、增加有機填料的添加量的方法等。但是,於利用該些方法使半導體用接著劑低彈性化的情況下,半導體用接著劑的操作性的惡化或熔融黏度的適當化變得困難,難以兼顧該些特性與封裝的低翹曲化。Here, as a method for achieving low warpage of the package, it is considered to reduce the elasticity of the adhesive for semiconductors. As methods of reducing the elasticity of the adhesive for semiconductors, methods of lowering the glass transition temperature of the polymer component, methods of reducing the amount of added inorganic fillers, methods of increasing the amount of added organic fillers, and the like are considered. However, when these methods are used to reduce the elasticity of a semiconductor adhesive, it becomes difficult to deteriorate the handleability of the semiconductor adhesive or to adjust the melt viscosity appropriately, and it is difficult to achieve a balance between these characteristics and low warpage of the package. .

本揭示為了解決所述課題而完成,目的在於提供一種可在抑制接著力及可靠性的降低的同時,實現所得的封裝的低翹曲化的半導體用接著劑、以及使用該半導體用接著劑的半導體裝置的製造方法及半導體裝置。 [解決課題之手段]The present disclosure was made to solve the above problems, and aims to provide an adhesive for semiconductors that can achieve low warpage of the resulting package while suppressing reductions in adhesive strength and reliability, and an adhesive using the adhesive for semiconductors. A method of manufacturing a semiconductor device and a semiconductor device. [Means to solve the problem]

為了達成所述目的,本揭示提供一種半導體用接著劑,含有重量平均分子量小於10000的樹脂、硬化劑、無機填料及矽酮橡膠填料。根據所述半導體用接著劑,藉由組合使用無機填料與矽酮橡膠填料作為填料,可在抑制接著力及可靠性的降低的同時,實現所得的封裝的低翹曲化。特別是藉由使用矽酮橡膠填料作為與無機填料併用的有機填料,可大幅度減少所得的封裝的翹曲。In order to achieve the above object, the present disclosure provides an adhesive for semiconductors, which contains a resin with a weight average molecular weight of less than 10,000, a hardener, an inorganic filler and a silicone rubber filler. According to the adhesive for semiconductors, by using an inorganic filler and a silicone rubber filler in combination as fillers, it is possible to achieve low warpage of the resulting package while suppressing reductions in adhesive strength and reliability. In particular, by using a silicone rubber filler as an organic filler in combination with an inorganic filler, the warpage of the resulting package can be significantly reduced.

所述矽酮橡膠填料的平均粒徑可為30 μm以下。該情況下,可在更充分地抑制接著力及可靠性的降低的同時,進一步減少所得的封裝的翹曲。The average particle size of the silicone rubber filler may be 30 μm or less. In this case, it is possible to further reduce the warpage of the resulting package while more fully suppressing the decrease in adhesive strength and reliability.

所述無機填料亦可含有二氧化矽填料。該情況下,可進一步提高接著力及可靠性。另外,無機填料與矽酮橡膠填料更容易均勻地分散,可以更高水準兼顧良好的接著力及可靠性與所得的封裝的低翹曲化。The inorganic filler may also contain silica filler. In this case, the adhesive force and reliability can be further improved. In addition, the inorganic filler and silicone rubber filler are more easily dispersed evenly, allowing a higher level of both good adhesion and reliability and low warpage of the resulting package.

所述半導體用接著劑亦可進而含有重量平均分子量為10000以上的高分子成分。該情況下,可提高半導體用接著劑的耐熱性及膜形成性。The adhesive for semiconductors may further contain a polymer component having a weight average molecular weight of 10,000 or more. In this case, the heat resistance and film formability of the semiconductor adhesive can be improved.

所述高分子成分的重量平均分子量可為30000以上。另外,所述高分子成分的玻璃轉移溫度亦可為100℃以下。若重量平均分子量為30000以上,則膜形成性變得良好。若玻璃轉移溫度為100℃以下,則對基板及半導體晶片的貼附性變得良好。The weight average molecular weight of the polymer component may be 30,000 or more. In addition, the glass transition temperature of the polymer component may be 100°C or lower. When the weight average molecular weight is 30,000 or more, film formability becomes good. When the glass transition temperature is 100° C. or lower, adhesion to the substrate and the semiconductor wafer becomes good.

所述半導體用接著劑亦可為膜狀。該情況下,可提高半導體用接著劑的操作性,且可提高封裝製造時的作業性及生產性。The adhesive agent for semiconductors may be in a film form. In this case, the workability of the adhesive for semiconductors can be improved, and the workability and productivity during package manufacturing can be improved.

以半導體用接著劑的固體成分總量為基準,所述半導體用接著劑中的所述矽酮橡膠填料的含量可為0.1質量%~20質量%。該情況下,可以更高水準兼顧良好的接著力及可靠性與所得的封裝的低翹曲化。Based on the total solid content of the adhesive for semiconductors, the content of the silicone rubber filler in the adhesive for semiconductors may be 0.1% by mass to 20% by mass. In this case, it is possible to achieve both good adhesion and reliability and low warpage of the resulting package at a higher level.

於所述半導體用接著劑中,所述矽酮橡膠填料的含量相對於所述無機填料的含量的質量比(矽酮橡膠填料的質量/無機填料的質量)可為0.05~0.5。該情況下,可以更高水準兼顧良好的接著力及可靠性與所得的封裝的低翹曲化。In the adhesive for semiconductors, the mass ratio of the content of the silicone rubber filler to the content of the inorganic filler (mass of the silicone rubber filler/mass of the inorganic filler) may be 0.05 to 0.5. In this case, it is possible to achieve both good adhesion and reliability and low warpage of the resulting package at a higher level.

另外,本揭示提供一種半導體裝置的製造方法,為製造半導體晶片及配線電路基板各自的連接部相互電性連接的半導體裝置、或者多個半導體晶片各自的連接部相互電性連接的半導體裝置的方法,所述半導體裝置的製造方法包括:使用所述半導體用接著劑對所述連接部的至少一部分進行密封的步驟。根據所述製造方法,可獲得半導體晶片與配線電路基板或半導體晶片之間的接著力及可靠性優異且翹曲減少的半導體裝置。In addition, the present disclosure provides a method of manufacturing a semiconductor device, which is a method of manufacturing a semiconductor device in which connecting portions of a semiconductor wafer and a printed circuit board are electrically connected to each other, or a semiconductor device in which connecting portions of a plurality of semiconductor wafers are electrically connected to each other. The method of manufacturing a semiconductor device includes the step of sealing at least part of the connection portion using the semiconductor adhesive. According to the manufacturing method, a semiconductor device can be obtained that has excellent adhesion and reliability between the semiconductor wafer and the printed circuit board or the semiconductor wafer and has reduced warpage.

進而,本揭示提供一種半導體裝置,包括:由半導體晶片及配線電路基板各自的連接部相互電性連接而成的連接結構、或者由多個半導體晶片各自的連接部相互電性連接而成的連接結構;以及將所述連接部的至少一部分密封的接著材料,所述接著材料包含所述半導體用接著劑的硬化物。所述半導體裝置成為半導體晶片與配線電路基板或半導體晶片之間的接著力及可靠性優異且翹曲減少的半導體裝置。 [發明的效果]Furthermore, the present disclosure provides a semiconductor device including a connection structure in which connection portions of a semiconductor chip and a printed circuit board are electrically connected to each other, or a connection structure in which connection portions of a plurality of semiconductor wafers are electrically connected to each other. A structure; and an adhesive material that seals at least part of the connection portion, the adhesive material including a cured product of the semiconductor adhesive. The semiconductor device has excellent adhesion and reliability between the semiconductor wafer and the printed circuit board or the semiconductor wafer, and has reduced warpage. [Effects of the invention]

根據本揭示,可提供一種可在抑制接著力及可靠性的降低的同時,實現所得的封裝的低翹曲化的半導體用接著劑、以及使用該半導體用接著劑的半導體裝置的製造方法及半導體裝置。According to the present disclosure, it is possible to provide an adhesive for semiconductors that can achieve low warpage of the resulting package while suppressing reductions in adhesive strength and reliability, as well as a method for manufacturing a semiconductor device using the adhesive for semiconductors, and a semiconductor. device.

以下,視情況,參照圖式對本揭示的適宜實施形態進行詳細說明。 再者,圖式中,對相同或相當部分標註相同符號,省略重覆說明。另外,上下左右等位置關係只要無特別說明,則視為基於圖式所示的位置關係。 進而,圖式的尺寸比率不限於圖示的比率。Hereinafter, suitable embodiments of the present disclosure will be described in detail with reference to the drawings as appropriate. In addition, in the drawings, the same or equivalent parts are denoted by the same symbols, and repeated explanations are omitted. In addition, unless otherwise specified, positional relationships such as up, down, left, and right are regarded as based on the positional relationships shown in the drawings. Furthermore, the dimensional ratio of the drawings is not limited to the ratio shown in the drawings.

本說明書中,使用「~」表示的數值範圍表示分別包含「~」的前後記載的數值作為最小值及最大值的範圍。於本說明書中階段性記載的數值範圍中,某一階段的數值範圍的上限值或下限值可與其他階段的數值範圍的上限值或下限值任意組合。於本說明書中記載的數值範圍中,所述數值範圍的上限值或下限值亦可替換成實施例所示的值。所謂「A或B」只要包含A及B中的任一者即可,亦可兩者都包含。本說明書中例示的材料只要無特別說明,則可單獨使用一種或者組合使用兩種以上。本說明書中,所謂「(甲基)丙烯酸」是指丙烯酸或與其對應的甲基丙烯酸。In this specification, the numerical range expressed using "~" means a range including the numerical values described before and after "~" as the minimum value and the maximum value, respectively. In the numerical ranges described in stages in this specification, the upper limit or lower limit of the numerical range in a certain stage can be arbitrarily combined with the upper limit or lower limit of the numerical range in other stages. In the numerical range described in this specification, the upper limit value or the lower limit value of the numerical range can also be replaced by the value shown in the embodiment. The so-called "A or B" only needs to include either A or B, or both. Unless otherwise specified, one type of materials exemplified in this specification may be used alone or two or more types may be used in combination. In this specification, "(meth)acrylic acid" means acrylic acid or its corresponding methacrylic acid.

<半導體用接著劑> 本實施形態的半導體用接著劑含有重量平均分子量小於10000的樹脂(以下視情況稱為「(a)成分」)、硬化劑(以下視情況稱為「(b)成分」)、無機填料(以下視情況稱為「(e)成分」)及有機填料(以下視情況稱為「(f)成分」)。另外,本實施形態的半導體用接著劑含有矽酮橡膠填料作為有機填料。進而,本實施形態的半導體用接著劑可視需要含有重量平均分子量為10000以上的高分子化合物(以下視情況稱為「(c)成分」)及/或助熔劑(以下視情況稱為「(d)成分」)。以下,對各成分進行說明。<Adhesives for semiconductors> The adhesive for semiconductors of this embodiment contains a resin with a weight average molecular weight of less than 10,000 (hereinafter referred to as "(a) component" as the case may be), a hardener (hereinafter referred to as "(b) component" as the case may be), and an inorganic filler (hereinafter referred to as "(b) component" as the case may be). (hereinafter referred to as "(e) component" as appropriate) and organic fillers (hereinafter referred to as "(f) component" as appropriate). In addition, the adhesive agent for semiconductors of this embodiment contains a silicone rubber filler as an organic filler. Furthermore, the adhesive agent for semiconductors of this embodiment may contain a polymer compound with a weight average molecular weight of 10,000 or more (hereinafter referred to as "(c) component" as the case may be) and/or a flux (hereinafter referred to as "(d) as the case may be"). )Element"). Each component is explained below.

(a)重量平均分子量小於10000的樹脂 作為(a)成分,並無特別限制,就耐熱性的觀點而言,較佳為與(b)成分的硬化劑反應的成分。作為(a)成分,較佳為分子內具有兩個以上的反應基者。作為(a)成分,例如可列舉:環氧樹脂、酚樹脂、醯亞胺樹脂、脲樹脂、三聚氰胺樹脂、矽酮樹脂、(甲基)丙烯酸化合物、乙烯基化合物。該些中,就耐熱性及保存穩定性優異的觀點而言,較佳為環氧樹脂、酚樹脂、醯亞胺樹脂,更佳為環氧樹脂、醯亞胺樹脂。該些(a)成分亦可單獨使用或者作為兩種以上的混合物或共聚物來使用。(a) Resins with a weight average molecular weight less than 10,000 The component (a) is not particularly limited, but from the viewpoint of heat resistance, a component that reacts with the curing agent of the component (b) is preferred. As component (a), one having two or more reactive groups in the molecule is preferred. Examples of the component (a) include epoxy resin, phenol resin, imide resin, urea resin, melamine resin, silicone resin, (meth)acrylic compound, and vinyl compound. Among these, from the viewpoint of excellent heat resistance and storage stability, epoxy resins, phenol resins, and amide imine resins are preferred, and epoxy resins and amide imine resins are more preferred. These (a) components may be used individually or as a mixture or copolymer of two or more types.

作為環氧樹脂,若為分子內具有兩個以上的環氧基者,則並無特別限制,例如可列舉:雙酚A型、雙酚F型、萘型、苯酚酚醛清漆型、甲酚酚醛清漆型、苯酚芳烷基型、聯苯型、三苯基甲烷型及二環戊二烯型等環氧樹脂、以及各種多官能環氧樹脂。環氧樹脂可單獨使用一種或者組合使用兩種以上。該些中,就耐熱性及操作性的觀點而言,較佳為雙酚F型環氧樹脂、苯酚酚醛清漆型環氧樹脂、甲酚酚醛清漆型環氧樹脂、聯苯型環氧樹脂及三苯基甲烷型環氧樹脂。The epoxy resin is not particularly limited as long as it has two or more epoxy groups in the molecule. Examples thereof include: bisphenol A type, bisphenol F type, naphthalene type, phenol novolak type, and cresol novolac type. Varnish type, phenol aralkyl type, biphenyl type, triphenylmethane type and dicyclopentadiene type epoxy resins, as well as various multi-functional epoxy resins. Epoxy resin can be used individually by 1 type or in combination of 2 or more types. Among these, from the viewpoint of heat resistance and workability, bisphenol F-type epoxy resin, phenol novolak-type epoxy resin, cresol novolak-type epoxy resin, biphenyl-type epoxy resin, and Triphenylmethane type epoxy resin.

作為醯亞胺樹脂,若為分子內具有兩個以上的醯亞胺基者,則並無特別限制,例如可列舉:耐地醯亞胺樹脂、烯丙基耐地醯亞胺樹脂、順丁烯二醯亞胺樹脂、醯胺醯亞胺樹脂、醯亞胺丙烯酸酯樹脂、各種多官能醯亞胺樹脂及各種聚醯亞胺樹脂。醯亞胺樹脂可單獨使用一種或者組合使用兩種以上。The acyl imine resin is not particularly limited as long as it has two or more acyl imine groups in the molecule. Examples thereof include: acyl imine-resistant resin, allyl acyl imine-resistant resin, cis-butyl imine resin, etc. Ethylenediimide resin, amideimine resin, amideimine acrylate resin, various multifunctional amideimine resins and various polyimide resins. The imine resin can be used individually by 1 type or in combination of 2 or more types.

就抑制於高溫下的連接時分解而產生揮發成分的觀點而言,於連接時的溫度為250℃的情況下,(a)成分較佳為使用250℃下的熱重量減少量係數為5%以下的樹脂,於連接時的溫度為300℃的情況下,較佳為使用300℃下的熱重量減少量係數為5%以下的樹脂。From the viewpoint of suppressing decomposition and generation of volatile components during connection at high temperatures, when the temperature during connection is 250°C, component (a) preferably uses a thermogravimetric reduction coefficient of 5% at 250°C. For the following resins, when the temperature during connection is 300°C, it is preferable to use resins whose thermogravimetric reduction coefficient at 300°C is 5% or less.

於使用環氧樹脂作為(a)成分的情況下,雙酚A型或雙酚F型的液狀環氧樹脂的1%熱重量減少溫度為250℃以下,因此有於高溫加熱時分解而產生揮發成分之虞。因此,較佳為使用於室溫(1氣壓、25℃)下為固體的環氧樹脂。於使用液狀環氧樹脂的情況下,較佳為與固體環氧樹脂組合使用。When using epoxy resin as component (a), the 1% thermogravimetric loss temperature of bisphenol A type or bisphenol F type liquid epoxy resin is 250°C or less, so it may be decomposed when heated to high temperatures. Concerns about volatile components. Therefore, it is preferable to use an epoxy resin that is solid at room temperature (1 atmosphere, 25°C). When liquid epoxy resin is used, it is preferably used in combination with solid epoxy resin.

(a)成分的重量平均分子量小於10000,就膜形成的觀點而言,較佳為小於10000,就熔融黏度的適當化的觀點而言,較佳為100以上。 因此,(a)成分的重量平均分子量較佳為100以上且小於10000,更佳為300以上且8000以下,進而較佳為300以上且5000以下。The weight average molecular weight of the component (a) is less than 10,000, preferably less than 10,000 from the viewpoint of film formation, and preferably 100 or more from the viewpoint of appropriate melt viscosity. Therefore, the weight average molecular weight of component (a) is preferably from 100 to 10,000, more preferably from 300 to 8,000, and even more preferably from 300 to 5,000.

以半導體用接著劑的固體成分總量為基準,(a)成分的含量例如為5質量%~75質量%,較佳為15質量%~60質量%,更佳為30質量%~50質量%。藉由將(a)成分的含量設為5質量%以上,接著力及可靠性優異,若為75質量%以下,則防止硬化物變得過硬,容易減少封裝的翹曲。Based on the total solid content of the semiconductor adhesive, the content of component (a) is, for example, 5% to 75% by mass, preferably 15% to 60% by mass, and more preferably 30% to 50% by mass. . By setting the content of component (a) to 5% by mass or more, adhesion and reliability are excellent, and if it is 75% by mass or less, the cured product is prevented from becoming too hard and warpage of the package is easily reduced.

(b)硬化劑 作為(b)硬化劑,例如可列舉:酚樹脂系硬化劑、酸酐系硬化劑、胺系硬化劑、咪唑系硬化劑及膦系硬化劑。若(b)成分包含酚性羥基、酸酐、胺類或咪唑類,則顯示出抑制於連接部中生成氧化膜的助熔活性,從而可使連接可靠性及絕緣可靠性提高。以下對各硬化劑加以說明。(b) Hardener Examples of (b) the curing agent include a phenol resin curing agent, an acid anhydride curing agent, an amine curing agent, an imidazole curing agent, and a phosphine curing agent. If the component (b) contains phenolic hydroxyl groups, acid anhydrides, amines, or imidazoles, it exhibits fluxing activity that suppresses the formation of oxide films in the connection portion, thereby improving connection reliability and insulation reliability. Each hardener is explained below.

(b-i)酚樹脂系硬化劑 作為酚樹脂系硬化劑,若為分子內具有兩個以上的酚性羥基者,則並無特別限制,可使用:苯酚酚醛清漆樹脂、甲酚酚醛清漆樹脂、苯酚芳烷基樹脂、甲酚萘酚甲醛縮聚物、三苯基甲烷型多官能酚樹脂及各種多官能酚樹脂等。該些可單獨使用或者作為兩種以上的混合物來使用。另外,液狀酚樹脂有於高溫加熱時分解而產生揮發成分之虞,因此理想的是使用於室溫(1氣壓、25℃)下為固體的酚樹脂。(b-i) Phenol resin hardener As the phenol resin hardener, if it has two or more phenolic hydroxyl groups in the molecule, it is not particularly limited, and can be used: phenol novolak resin, cresol novolac resin, phenol aralkyl resin, cresol naphthalene Phenol formaldehyde condensation polymer, triphenylmethane type multifunctional phenol resin and various multifunctional phenol resins, etc. These can be used individually or as a mixture of two or more types. In addition, liquid phenol resins may decompose when heated at high temperatures to produce volatile components, so it is ideal to use phenol resins that are solid at room temperature (1 atmosphere, 25°C).

就使硬化性、接著性及保存穩定性等良好的觀點而言,(b-i)酚樹脂系硬化劑相對於所述(a)成分的當量比(酚性羥基/(a)成分的反應基的莫耳比)較佳為0.3~1.5,更佳為0.4~1.0,進而較佳為0.5~1.0。若當量比為0.3以上,則有硬化性提高,接著力提高的傾向,若為1.5以下,則不會過剩地殘存未反應的酚性羥基,吸水率被抑制為低值,有絕緣可靠性提高的傾向。酚性羥基顯示出去除氧化膜的助熔活性,因此藉由半導體用接著劑含有酚樹脂系硬化劑,可提高連接性、可靠性。From the viewpoint of improving curability, adhesion, storage stability, etc., the equivalent ratio (phenolic hydroxyl group/reactive group of the component (a)) of the (b-i) phenolic resin-based curing agent to the component (a) molar ratio) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, still more preferably 0.5 to 1.0. If the equivalent ratio is 0.3 or more, the hardening properties tend to be improved and the adhesion force will be improved. If it is 1.5 or less, unreacted phenolic hydroxyl groups will not remain excessively, the water absorption rate will be suppressed to a low value, and the insulation reliability will be improved. tendency. Phenolic hydroxyl groups show fluxing activity that removes oxide films. Therefore, when a semiconductor adhesive contains a phenolic resin-based hardener, connectivity and reliability can be improved.

(b-ii)酸酐系硬化劑 作為酸酐系硬化劑,例如可使用:甲基環己烷四羧酸二酐、偏苯三甲酸酐、均苯四甲酸酐、二苯甲酮四羧酸二酐及乙二醇雙偏苯三甲酸酐酯等。該些可單獨使用或者作為兩種以上的混合物來使用。另外,液狀酸酐有於高溫加熱時分解而產生揮發成分之虞,因此理想的是使用於室溫(1氣壓、25℃)下為固體的酸酐。(b-ii) Acid anhydride hardener Examples of acid anhydride-based hardeners that can be used include: methylcyclohexanetetracarboxylic dianhydride, trimellitic anhydride, pyromellitic anhydride, benzophenone tetracarboxylic dianhydride, and ethylene glycol bis-trimellitic anhydride. Ester etc. These can be used individually or as a mixture of two or more types. In addition, liquid acid anhydrides may decompose when heated at high temperatures to produce volatile components, so it is ideal to use acid anhydrides that are solid at room temperature (1 atmosphere, 25°C).

就使硬化性、接著性及保存穩定性等良好的觀點而言,(b-ii)酸酐系硬化劑相對於所述(a)成分的當量比(酸酐基/(a)成分的反應基的莫耳比)較佳為0.3~1.5,更佳為0.4~1.0,進而較佳為0.5~1.0。若當量比為0.3以上,則有硬化性提高,接著力提高的傾向,若為1.5以下,則不會過剩地殘存未反應的酸酐,吸水率被抑制為低值,有絕緣可靠性提高的傾向。酸酐顯示出去除氧化膜的助熔活性,因此藉由半導體用接著劑含有酸酐系硬化劑,可提高連接性、可靠性。From the viewpoint of improving the curability, adhesion, storage stability, etc., the equivalent ratio (acid anhydride group/reactive group of the component (a)) of the acid anhydride-based curing agent (b-ii) to the component (a) molar ratio) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, still more preferably 0.5 to 1.0. If the equivalent ratio is 0.3 or more, the hardenability and adhesion force tend to be improved. If it is 1.5 or less, unreacted acid anhydride will not remain excessively, the water absorption rate will be suppressed to a low value, and the insulation reliability will tend to be improved. . Acid anhydrides exhibit fluxing activity that removes oxide films. Therefore, when a semiconductor adhesive contains an acid anhydride-based hardener, connectivity and reliability can be improved.

(b-iii)胺系硬化劑 作為胺系硬化劑,可使用二氰二胺等。另外,液狀胺有於高溫加熱時分解而產生揮發成分之虞,因此理想的是使用於室溫(1氣壓、25℃)下為固體的胺。(b-iii) Amine hardener As the amine-based hardener, dicyandiamide or the like can be used. In addition, liquid amines may decompose during high-temperature heating to produce volatile components, so it is ideal to use amines that are solid at room temperature (1 atmosphere, 25°C).

就使硬化性、接著性及保存穩定性等良好的觀點而言,(b-iii)胺系硬化劑相對於所述(a)成分的當量比(胺/(a)成分的反應基的莫耳比)較佳為0.3~1.5,更佳為0.4~1.0,進而較佳為0.5~1.0。若當量比為0.3以上,則有硬化性提高,接著力提高的傾向,若為1.5以下,則不會過剩地殘存未反應的胺,吸水率被抑制為低值,有絕緣可靠性提高的傾向。胺類顯示出去除氧化膜的助熔活性,因此藉由半導體用接著劑含有胺系硬化劑,可提高連接性、可靠性。From the viewpoint of improving curability, adhesion, storage stability, etc., the equivalent ratio of (b-iii) the amine-based curing agent to the component (a) (the molar ratio of the reactive group of the amine/component (a) ear ratio) is preferably 0.3 to 1.5, more preferably 0.4 to 1.0, further preferably 0.5 to 1.0. If the equivalent ratio is 0.3 or more, the hardenability will be improved and the adhesive force will tend to be improved. If it is 1.5 or less, unreacted amine will not remain excessively, the water absorption rate will be suppressed to a low value, and the insulation reliability will tend to be improved. . Amines exhibit fluxing activity that removes oxide films. Therefore, when a semiconductor adhesive contains an amine-based hardener, connectivity and reliability can be improved.

(b-iv)咪唑系硬化劑(所含有的氮原子為三級氮原子) 作為咪唑系硬化劑,可列舉:1-苄基-2-甲基咪唑、1-苄基-2-苯基咪唑、1-氰基乙基-2-十一烷基咪唑、1-氰基乙基-2-苯基咪唑、1-氰基乙基-2-十一烷基咪唑偏苯三甲酸酯、1-氰基乙基-2-苯基咪唑鎓偏苯三甲酸酯、2,4-二胺基-6-[2'-甲基咪唑基-(1')]-乙基-均三嗪、2,4-二胺基-6-[2'-十一烷基咪唑基-(1')]-乙基-均三嗪、2,4-二胺基-6-[2'-乙基-4'-甲基咪唑基-(1')]-乙基-均三嗪、2,4-二胺基-6-[2'-甲基咪唑基-(1')]-乙基-均三嗪異三聚氰酸加成物、2-苯基咪唑異三聚氰酸加成物、環氧樹脂與咪唑類的加成物等。該些中,就使硬化性、接著性及保存穩定性等良好的觀點而言,較佳為1-氰基乙基-2-十一烷基咪唑、1-氰基乙基-2-苯基咪唑、1-氰基乙基-2-十一烷基咪唑偏苯三甲酸酯、1-氰基乙基-2-苯基咪唑鎓偏苯三甲酸酯、2,4-二胺基-6-[2'-甲基咪唑基-(1')]-乙基-均三嗪、2,4-二胺基-6-[2'-乙基-4'-甲基咪唑基-(1')]-乙基-均三嗪、2,4-二胺基-6-[2'-甲基咪唑基-(1')]-乙基-均三嗪異三聚氰酸加成物、2-苯基咪唑異三聚氰酸加成物。該些可單獨使用或者組合使用兩種以上。另外,亦可使用將該些進行微膠囊化而提高潛在性的潛在性硬化劑。(b-iv) Imidazole hardener (the nitrogen atoms contained are tertiary nitrogen atoms) Examples of imidazole-based hardeners include: 1-benzyl-2-methylimidazole, 1-benzyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole, and 1-cyano Ethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2, 4-Diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine Azine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isotripolymer Cyanic acid adducts, adducts of epoxy resin and imidazoles, etc. Among these, from the viewpoint of improving hardenability, adhesion, storage stability, etc., 1-cyanoethyl-2-undecylimidazole and 1-cyanoethyl-2-benzene are preferred. imidazole, 1-cyanoethyl-2-undecylimidazole trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino- 6-[2'-Methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-( 1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid addition substance, 2-phenylimidazole isocyanuric acid adduct. These can be used individually or in combination of 2 or more types. In addition, a latent hardening agent that can be microencapsulated to improve the potency can also be used.

相對於(a)成分100質量份,(b-iv)咪唑系硬化劑的含量較佳為0.1質量份~20質量份,更佳為0.1質量份~10質量份。若該含量為0.1質量份以上,則有硬化性提高的傾向,若為20質量份以下,則於金屬接合形成之前半導體用接著劑不會硬化,有不易產生連接不良的傾向。咪唑系硬化劑可單獨作為(b)硬化劑使用,亦可與所述(b-i)~(b-iii)的硬化劑一起作為硬化促進劑使用。The content of the (b-iv) imidazole hardener is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass relative to 100 parts by mass of the component (a). If the content is 0.1 parts by mass or more, the curability tends to be improved. If the content is 20 parts by mass or less, the semiconductor adhesive does not harden before metal bonding is formed, and connection defects tend to be less likely to occur. The imidazole-based hardening agent may be used alone as the hardening agent (b) or may be used as a hardening accelerator together with the hardening agents (b-i) to (b-iii) described above.

(b-v)膦系硬化劑 作為膦系硬化劑,可列舉:三苯基膦、四苯基鏻四苯基硼酸鹽、四苯基鏻四(4-甲基苯基)硼酸鹽、四苯基鏻(4-氟苯基)硼酸鹽等。(b-v) Phosphine hardener Examples of phosphine-based hardeners include triphenylphosphine, tetraphenylphosphonium tetraphenylborate, tetraphenylphosphonium tetrakis(4-methylphenyl)borate, tetraphenylphosphonium(4-fluorophenyl) ) borate, etc.

相對於(a)成分100質量份,(b-v)膦系硬化劑的含量較佳為0.1質量份~10質量份,更佳為0.1質量份~5質量份。若膦系硬化劑的含量為0.1質量份以上,則有硬化性提高的傾向,若為10質量份以下,則於金屬接合形成之前膜狀接著劑不會硬化,有不易產生連接不良的傾向。The content of the (b-v) phosphine-based hardener is preferably 0.1 to 10 parts by mass, more preferably 0.1 to 5 parts by mass relative to 100 parts by mass of the component (a). If the content of the phosphine-based curing agent is 0.1 parts by mass or more, the curability tends to be improved. If it is 10 parts by mass or less, the film-like adhesive does not harden before metal bonding is formed, and connection failures tend to be less likely to occur.

酚樹脂系硬化劑、酸酐系硬化劑及胺系硬化劑分別可單獨使用一種或者作為兩種以上的混合物來使用。咪唑系硬化劑及膦系硬化劑分別可單獨使用,亦可與酚樹脂系硬化劑、酸酐系硬化劑或胺系硬化劑一併使用。Each of the phenolic resin-based hardener, the acid anhydride-based hardener, and the amine-based hardener can be used individually by one type or as a mixture of two or more types. The imidazole-based hardener and the phosphine-based hardener can be used alone or together with a phenol resin-based hardener, an acid anhydride-based hardener, or an amine-based hardener.

(c)重量平均分子量10000以上的高分子成分 作為(c)重量平均分子量10000以上的高分子成分,可列舉:苯氧基樹脂、聚醯亞胺樹脂、聚醯胺樹脂、聚碳二醯亞胺樹脂、氰酸酯樹脂、丙烯酸樹脂、聚酯樹脂、聚乙烯樹脂、聚醚碸樹脂、聚醚醯亞胺樹脂、聚乙烯縮醛樹脂、胺基甲酸酯樹脂、丙烯酸橡膠等。該些中,就耐熱性及膜形成性優異的方面而言,理想的是苯氧基樹脂、聚醯亞胺樹脂、丙烯酸橡膠、氰酸酯樹脂、聚碳二醯亞胺樹脂等,更佳為苯氧基樹脂、聚醯亞胺樹脂、丙烯酸橡膠,進而較佳為苯氧基樹脂。該些高分子成分可單獨使用或者作為兩種以上的混合物或共聚物使用。(c) Polymer components with a weight average molecular weight of more than 10,000 (c) Polymer components having a weight average molecular weight of 10,000 or more include: phenoxy resin, polyamide resin, polyamide resin, polycarbodiimide resin, cyanate ester resin, acrylic resin, polyamide resin, Ester resin, polyethylene resin, polyether resin, polyetherimide resin, polyvinyl acetal resin, urethane resin, acrylic rubber, etc. Among these, phenoxy resin, polyimide resin, acrylic rubber, cyanate ester resin, polycarbodiimide resin, etc. are preferable from the viewpoint of excellent heat resistance and film formation properties, and more preferred They are phenoxy resin, polyimide resin, and acrylic rubber, and phenoxy resin is more preferred. These polymer components can be used alone or as a mixture or copolymer of two or more types.

(c)成分、(a)成分與(b)成分的質量比並無特別限制,就使膜形成性及利用旋塗等的成膜性良好的觀點而言,相對於(c)成分1質量份,(a)成分及(b)成分的合計質量較佳為0.01質量份~5質量份,更佳為0.1質量份~4質量份,進而較佳為0.1質量份~3質量份。若該質量比為0.01質量份以上,則有可抑制半導體用接著劑的硬化性的降低、可抑制接著力的降低的傾向,若為5質量份以下,則有可使膜形成性及成膜性良好的傾向。The mass ratio of component (c), component (a), and component (b) is not particularly limited. From the viewpoint of improving film-forming properties and film-forming properties by spin coating, etc., 1 mass of component (c) parts, the total mass of component (a) and component (b) is preferably 0.01 to 5 parts by mass, more preferably 0.1 to 4 parts by mass, and still more preferably 0.1 to 3 parts by mass. If the mass ratio is 0.01 parts by mass or more, the decrease in the curability of the semiconductor adhesive and the decrease in the adhesive force tend to be suppressed. If the mass ratio is 5 parts by mass or less, the film formability and film formation tend to be improved. Good sexual tendencies.

作為(c)成分使用的聚醯亞胺樹脂例如可利用公知的方法使四羧酸二酐與二胺進行縮合反應而獲得。更具體而言,於有機溶媒中,將四羧酸二酐與二胺以等莫耳或大致等莫耳混合(各成分的添加順序任意),於反應溫度80℃以下、較佳為0℃~60℃下進行加成反應。隨著反應的進行,反應液的黏度逐漸上升,生成作為聚醯亞胺的前驅物的聚醯胺酸。再者,為了抑制半導體用接著劑的各種特性的降低,較佳為所述四羧酸二酐利用乙酸酐進行再結晶精製處理。The polyimide resin used as component (c) can be obtained by condensing tetracarboxylic dianhydride and diamine by a known method, for example. More specifically, in an organic solvent, tetracarboxylic dianhydride and diamine are mixed in equimolar or approximately equimolar amounts (the order of addition of each component is arbitrary), and the reaction temperature is 80°C or lower, preferably 0°C. The addition reaction proceeds at ~60°C. As the reaction proceeds, the viscosity of the reaction solution gradually increases, and polyamic acid, which is the precursor of polyimide, is generated. Furthermore, in order to suppress deterioration in various characteristics of the semiconductor adhesive, it is preferable that the tetracarboxylic dianhydride is subjected to recrystallization purification treatment using acetic anhydride.

所述聚醯胺酸亦可藉由於50℃~80℃的溫度下加熱使其解聚來調整其分子量。The molecular weight of the polyamide can also be adjusted by depolymerizing it by heating at a temperature of 50°C to 80°C.

聚醯亞胺樹脂可使所述反應產物(聚醯胺酸)脫水閉環而獲得。脫水閉環可利用進行加熱處理的熱閉環法或使用脫水劑的化學閉環法進行。Polyimide resin can be obtained by dehydrating and ring-closing the reaction product (polyamide acid). Dehydration loop closure can be performed by a thermal loop closure method using heat treatment or a chemical loop closure method using a dehydrating agent.

就使對基板及半導體晶片的貼附性良好的觀點而言,(c)成分的玻璃轉移溫度(Tg)較佳為100℃以下,更佳為75℃以下。若Tg為100℃以下,則利用半導體用接著劑容易將形成於半導體晶片上的凸塊或者形成於基板上的電極或配線圖案等的凹凸填埋,有可防止氣泡的殘存、抑制孔隙(void)的產生的傾向。再者,所述Tg是使用示差掃描熱量計(珀金埃爾默(PerkinElmer)公司製造,DSC-7型),在樣品量10 mg、升溫速度5℃/min、測定環境:空氣的條件下測定時的Tg。From the viewpoint of improving the adhesion to the substrate and the semiconductor wafer, the glass transition temperature (Tg) of the component (c) is preferably 100°C or lower, more preferably 75°C or lower. If Tg is 100°C or less, bumps formed on a semiconductor wafer or irregularities such as electrodes or wiring patterns formed on a substrate can be easily filled with the semiconductor adhesive, thereby preventing bubbles from remaining and suppressing voids. ) the tendency to produce. In addition, the Tg was measured using a differential scanning calorimeter (DSC-7 model manufactured by PerkinElmer) under the conditions of sample amount 10 mg, temperature rise rate 5°C/min, and measurement environment: air. Tg at the time of measurement.

(c)成分的重量平均分子量以聚苯乙烯換算計為10000以上,為了單獨顯示出良好的膜形成性,較佳為20000以上,更佳為30000以上,進而較佳為40000以上。於重量平均分子量小於10000的情況下,有膜形成性降低之虞。另外,考慮到流動性,(c)成分的重量平均分子量例如為100萬以下,較佳為50萬以下。The weight average molecular weight of the component (c) is 10,000 or more in terms of polystyrene. In order to exhibit good film-forming properties alone, it is preferably 20,000 or more, more preferably 30,000 or more, and still more preferably 40,000 or more. When the weight average molecular weight is less than 10,000, film formation properties may be reduced. In addition, taking fluidity into consideration, the weight average molecular weight of component (c) is, for example, 1 million or less, preferably 500,000 or less.

本說明書中,所謂重量平均分子量是指使用高效液相層析法(島津製作所製造的C-R4A)以聚苯乙烯換算測定時的重量平均分子量。In this specification, the weight average molecular weight refers to the weight average molecular weight when measured in terms of polystyrene using high performance liquid chromatography (C-R4A manufactured by Shimadzu Corporation).

(c)成分與(a)成分的含量的比並無特別限制,就良好地保持膜狀的觀點而言,相對於(c)成分1質量份,較佳為(a)成分為0.01質量份~5質量份,更佳為0.1質量份~2質量份。若該含量的比為0.01質量份以上,則有可抑制半導體用接著劑的硬化性的降低、可抑制接著力的降低的傾向,若為5質量份以下,則有可使膜形成性及成膜性良好的傾向。The ratio of the content of component (c) to component (a) is not particularly limited, but from the viewpoint of maintaining a good film shape, it is preferably 0.01 part by mass of component (a) relative to 1 part by mass of component (c). ~5 parts by mass, more preferably 0.1-2 parts by mass. If the ratio of the content is 0.01 parts by mass or more, the decrease in the curability of the semiconductor adhesive and the decrease in the adhesive force tend to be suppressed. If the ratio is 5 parts by mass or less, the film formability and composition may be reduced. Good film properties.

(d)助熔劑 半導體用接著劑可含有(d)助熔劑、即、作為顯示出助熔活性(去除氧化物及雜質的活性)的化合物的助熔活性劑。作為助熔劑,例如可列舉如咪唑類及胺類般具有非共價電子對的含氮化合物、羧酸類、苯酚類及醇類。再者,與醇類相比,如羧酸類般的有機酸類更強烈地顯現出助熔活性,容易提高連接性。(d) Flux The adhesive for semiconductors may contain (d) a flux, that is, a flux activator that is a compound showing fluxing activity (activity for removing oxides and impurities). Examples of the flux include nitrogen-containing compounds having non-covalent electron pairs such as imidazoles and amines, carboxylic acids, phenols and alcohols. In addition, organic acids such as carboxylic acids exhibit fluxing activity more strongly than alcohols and can easily improve connectivity.

就顯現出助熔活性並提高連接性的觀點而言,以半導體用接著劑的固體成分總量為基準,(d)成分的含量較佳為0.1質量%~5質量%,更佳為1質量%~5質量%。From the viewpoint of exhibiting fluxing activity and improving connectivity, the content of component (d) is preferably 0.1 mass % to 5 mass %, more preferably 1 mass %, based on the total solid content of the semiconductor adhesive. %~5 mass%.

(e)無機填料 本實施形態的半導體用接著劑含有無機填料作為(e)成分。藉由含有(e)成分,可控制半導體用接著劑的黏度及硬化物的物性,可抑制將半導體晶片與基板連接時的孔隙的產生及吸濕率。另外,藉由含有(e)成分,半導體用接著劑可獲得優異的接著力,且可提高耐回焊性及耐濕性等可靠性。(e) Inorganic filler The adhesive agent for semiconductors of this embodiment contains an inorganic filler as (e) component. By containing the component (e), the viscosity of the semiconductor adhesive and the physical properties of the cured product can be controlled, and the generation of voids and the moisture absorption rate when connecting the semiconductor wafer and the substrate can be suppressed. In addition, by containing the component (e), the adhesive agent for semiconductors can obtain excellent adhesive strength, and can improve reliability such as reflow resistance and moisture resistance.

作為(e)成分,例如可列舉絕緣性無機填料及晶鬚。作為絕緣性無機填料的材質,可列舉玻璃、二氧化矽、氧化鋁、二氧化矽-氧化鋁、氧化鈦、雲母、氮化硼等,其中,較佳為二氧化矽、氧化鋁、二氧化矽-氧化鋁、氧化鈦、氮化硼等,更佳為二氧化矽、氧化鋁、氮化硼,進而較佳為二氧化矽。作為晶鬚的材質,可列舉硼酸鋁、鈦酸鋁、氧化鋅、矽酸鈣、硫酸鎂、氮化硼等。Examples of the component (e) include insulating inorganic fillers and whiskers. Examples of materials for the insulating inorganic filler include glass, silica, alumina, silica-alumina, titanium oxide, mica, boron nitride, and the like. Among them, silica, alumina, and boron nitride are preferred. Silicon - aluminum oxide, titanium oxide, boron nitride, etc., more preferably silicon dioxide, aluminum oxide, boron nitride, and still more preferably silicon dioxide. Examples of whisker materials include aluminum borate, aluminum titanate, zinc oxide, calcium silicate, magnesium sulfate, boron nitride, and the like.

就分散性及接著力提高的觀點而言,(e)成分較佳為表面處理填料。作為表面處理,可列舉縮水甘油基系(環氧系)、胺系、苯基系、苯基胺基系、丙烯酸系、乙烯基系等。From the viewpoint of improving dispersion and adhesion, component (e) is preferably a surface treatment filler. Examples of surface treatments include glycidyl-based (epoxy-based), amine-based, phenyl-based, phenylamino-based, acrylic-based, vinyl-based, and the like.

作為表面處理,就表面處理的容易性而言,較佳為利用環氧矽烷系、胺基矽烷系、丙烯酸矽烷系等矽烷化合物進行的矽烷處理。作為表面處理劑,就分散性及流動性優異且進一步提高接著力的觀點而言,較佳為縮水甘油基系、苯基胺基系、(甲基)丙烯酸系的化合物。作為表面處理劑,就保存穩定性的觀點而言,較佳為苯基系、(甲基)丙烯酸系的化合物。As surface treatment, in terms of ease of surface treatment, silane treatment using silane compounds such as epoxy silane type, amino silane type, and acrylic silane type is preferred. As the surface treatment agent, glycidyl-based, phenylamino-based, or (meth)acrylic-based compounds are preferred from the viewpoint of excellent dispersion and fluidity and further improvement in adhesive strength. As the surface treatment agent, from the viewpoint of storage stability, phenyl-based or (meth)acrylic-based compounds are preferred.

關於(e)成分的粒徑,就防止覆晶連接時的含入的觀點而言,平均粒徑較佳為1.5 μm以下,就視認性(透明性)的觀點而言,平均粒徑更佳為1.0 μm以下。(e)成分的平均粒徑例如可藉由濕式-乾式粒度分佈測定裝置(貝克曼-庫爾特(beckman-coulter)製造,LS13 320)測定。Regarding the particle diameter of component (e), from the viewpoint of preventing inclusion during flip-chip connection, the average particle diameter is preferably 1.5 μm or less, and from the viewpoint of visibility (transparency), the average particle diameter is even more preferable. is less than 1.0 μm. (e) The average particle diameter of the component can be measured, for example, with a wet-dry particle size distribution measuring device (LS13 320, manufactured by Beckman-Coulter).

該些(e)成分亦可單獨使用或者作為兩種以上的混合體使用。關於(e)成分的形狀,並無特別限制。These (e) components may be used individually or as a mixture of two or more types. The shape of component (e) is not particularly limited.

以半導體用接著劑的固體成分總量為基準,(e)成分的含量較佳為20質量%~60質量%,更佳為30質量%~50質量%。若該含量為20質量%以上、特別是30質量%以上,則有可進一步抑制孔隙產生及吸濕率、可進一步提高接著力以及耐回焊性及耐濕性等可靠性的傾向。另一方面,若含量為60質量%以下、特別是50質量%以下,則有容易減少所得的封裝的翹曲且容易防止覆晶連接時的含入的傾向。Based on the total solid content of the semiconductor adhesive, the content of component (e) is preferably 20 to 60 mass%, more preferably 30 to 50 mass%. If the content is 20% by mass or more, especially 30% by mass or more, the generation of voids and the moisture absorption rate tend to be further suppressed, and reliability such as adhesive strength, reflow resistance, and moisture resistance tend to be further improved. On the other hand, if the content is 60% by mass or less, especially 50% by mass or less, the warpage of the resulting package tends to be easily reduced and inclusion during flip-chip connection tends to be easily prevented.

(f)有機填料 本實施形態的半導體用接著劑含有有機填料作為(f)成分。藉由含有(f)成分,可控制半導體用接著劑的黏度及硬化物的物性,可抑制將半導體晶片與基板連接時的孔隙的產生及吸濕率。(f) Organic filler The adhesive agent for semiconductors of this embodiment contains an organic filler as (f) component. By containing the component (f), the viscosity of the semiconductor adhesive and the physical properties of the cured product can be controlled, and the generation of voids and the moisture absorption rate when connecting the semiconductor wafer and the substrate can be suppressed.

作為有機填料的材質,例如可列舉聚胺基甲酸酯、聚醯亞胺、矽酮、甲基丙烯酸甲酯樹脂及甲基丙烯酸甲酯-丁二烯-苯乙烯共聚樹脂(Methylmethacrylate Butadiene Styrene,MBS)。(f)成分與(e)成分相比,可於260℃等高溫下對半導體用接著劑及其硬化物賦予柔軟性,因此適於提高耐回焊性及耐溫度循環性。另外,由於賦予柔軟性,因此對提高膜形成性亦有效。Examples of organic filler materials include polyurethane, polyimide, silicone, methyl methacrylate resin, and methyl methacrylate-butadiene-styrene copolymer resin (Methylmethacrylate Butadiene Styrene, MBS). Compared with the component (e), the component (f) can impart flexibility to the semiconductor adhesive and its cured product at high temperatures such as 260°C, and is therefore suitable for improving reflow resistance and temperature cycle resistance. In addition, since it imparts flexibility, it is also effective in improving film formability.

該些(f)成分亦可單獨使用或者作為兩種以上的混合體使用。關於(f)成分的形狀,並無特別限制。These (f) components may be used individually or as a mixture of 2 or more types. The shape of component (f) is not particularly limited.

本實施形態的半導體用接著劑含有矽酮橡膠填料作為(f)成分。藉由半導體用接著劑含有矽酮橡膠填料,可實現所得的封裝的低翹曲化。The adhesive agent for semiconductors of this embodiment contains a silicone rubber filler as the (f) component. When the adhesive for semiconductors contains a silicone rubber filler, the resulting package can have low warpage.

矽酮橡膠填料只要是含有矽酮橡膠作為填料的構成成分的填料即可,可為僅包含矽酮橡膠的填料,亦可為與其他成分複合化的填料。矽酮橡膠填料可為具有核-殼型結構的粒子。作為核-殼型的結構,可列舉具有核層(核材料)以及以被覆核層的方式設置的殼層(表面層)的結構。核層與殼層的組成可相同亦可不同。再者,核層與殼層未必具有清楚的邊界線。作為矽酮橡膠填料,例如可使用核層由矽酮橡膠粒子構成、殼層由矽酮橡膠粒子以外的其他成分構成的複合粒子。作為此種複合粒子,較佳為可列舉核層由矽酮橡膠粒子構成、殼層由具有比核層的矽酮橡膠粒子高的玻璃轉移溫度及彈性係數的矽酮樹脂構成的矽酮複合粉末。此種矽酮複合粉末可藉由殼層來抑制核層的矽酮橡膠粒子因溶劑或半導體用接著劑的構成材料發生膨潤而在矽酮橡膠粒子彼此之間形成凝聚體。The silicone rubber filler only needs to be a filler containing silicone rubber as a constituent component of the filler, and may be a filler containing only silicone rubber or a filler compounded with other components. The silicone rubber filler may be particles with a core-shell structure. Examples of a core-shell type structure include a structure having a core layer (core material) and a shell layer (surface layer) provided to cover the core layer. The compositions of the core layer and the shell layer may be the same or different. Furthermore, the core layer and the shell layer may not have a clear boundary line. As the silicone rubber filler, for example, composite particles in which the core layer is composed of silicone rubber particles and the shell layer is composed of components other than silicone rubber particles can be used. Preferable examples of such composite particles include a silicone composite powder in which the core layer is composed of silicone rubber particles and the shell layer is composed of a silicone resin having a higher glass transition temperature and elastic coefficient than the silicone rubber particles of the core layer. . The shell layer of this silicone composite powder can prevent the silicone rubber particles in the core layer from swelling due to the solvent or the constituent material of the semiconductor adhesive, thereby preventing the formation of agglomerates between the silicone rubber particles.

矽酮橡膠填料的平均粒徑較佳為0.1 μm~50 μm,更佳為0.1 μm~30 μm,進而較佳為0.1 μm~10 μm。若平均粒徑為50 μm以下,則有安裝時的連接性變得良好的傾向。矽酮橡膠填料的平均粒徑例如可藉由濕式-乾式粒度分佈測定裝置(貝克曼-庫爾特(beckman-coulter)製造,LS13 320)測定。The average particle size of the silicone rubber filler is preferably 0.1 μm to 50 μm, more preferably 0.1 μm to 30 μm, and further preferably 0.1 μm to 10 μm. When the average particle diameter is 50 μm or less, the connectivity during mounting tends to be good. The average particle size of the silicone rubber filler can be measured, for example, by a wet-dry particle size distribution measuring device (LS13 320 manufactured by Beckman-Coulter).

以半導體用接著劑的固體成分總量為基準,矽酮橡膠填料的含量較佳為0.1質量%~20質量%,更佳為1質量%~18質量%,進而較佳為3質量%~15質量%。若該含量為0.1質量%以上,則有容易低彈性化的傾向,若為20質量%以下,則有容易使熔融黏度適當化的傾向。Based on the total solid content of the semiconductor adhesive, the content of the silicone rubber filler is preferably 0.1% to 20% by mass, more preferably 1% to 18% by mass, and further preferably 3% to 15% by mass. Mass %. If the content is 0.1% by mass or more, the elasticity tends to be low, and if it is 20% by mass or less, the melt viscosity tends to be appropriately adjusted.

就更充分地獲得本揭示的效果的觀點而言,以(f)成分總量為基準,矽酮橡膠填料的含量在(f)成分中所佔的比例較佳為50質量%以上,更佳為80質量%以上。再者,矽酮橡膠填料的含量的比例亦可為100質量%。From the viewpoint of obtaining the effects of the present disclosure more fully, the proportion of the content of the silicone rubber filler in component (f) is preferably 50 mass % or more based on the total amount of component (f), and more preferably It is more than 80 mass%. Furthermore, the content ratio of the silicone rubber filler may also be 100% by mass.

矽酮橡膠填料的含量相對於(e)成分的含量的質量比(矽酮橡膠填料的質量/無機填料的質量)較佳為0.05~0.5,更佳為0.08~0.4,進而較佳為0.1~0.3。藉由使該質量比為所述範圍內,可以更高水準兼顧良好的接著力及可靠性與所得的封裝的低翹曲化。The mass ratio of the content of the silicone rubber filler to the content of the component (e) (mass of the silicone rubber filler/mass of the inorganic filler) is preferably 0.05 to 0.5, more preferably 0.08 to 0.4, and still more preferably 0.1 to 0.1. 0.3. By setting the mass ratio within the above range, it is possible to achieve both good adhesion and reliability and low warpage of the resulting package at a higher level.

以半導體用接著劑的固體成分整體為基準,(e)成分及(f)成分的合計含量較佳為30質量%~90質量%,更佳為40質量%~80質量%。若含量為30質量%以上,則有可更充分地提高接著力的傾向。若含量為90質量%以下,則有可抑制黏度變高而產生半導體用接著劑的流動性的降低及填料向連接部的含入(陷入(trapping)),可獲得良好的連接可靠性的傾向。Based on the solid content of the entire semiconductor adhesive, the total content of component (e) and component (f) is preferably 30% by mass to 90% by mass, more preferably 40% by mass to 80% by mass. If the content is 30% by mass or more, the adhesive force tends to be more fully improved. If the content is 90% by mass or less, it is possible to suppress the decrease in fluidity of the semiconductor adhesive due to an increase in viscosity and the inclusion (trapping) of the filler into the connection part, thereby tending to obtain good connection reliability. .

就絕緣可靠性的觀點而言,填料較佳為絕緣性。半導體用接著劑較佳為不含銀填料、焊料填料等導電性金屬填料。不含導電性填料(導電性粒子)的半導體用接著劑(電路連接材料)亦有時被稱為非導電膜(Non-Conductive-FILM,NCF)或非導電膠(Non-Conductive-Paste,NCP)。本實施形態的半導體用接著劑可適宜地用作NCF或NCP。From the viewpoint of insulation reliability, the filler is preferably insulating. The adhesive for semiconductors preferably does not contain conductive metal fillers such as silver fillers and solder fillers. Semiconductor adhesives (circuit connection materials) that do not contain conductive fillers (conductive particles) are sometimes called non-conductive film (Non-Conductive-FILM, NCF) or non-conductive paste (Non-Conductive-Paste, NCP) ). The adhesive agent for semiconductors of this embodiment can be suitably used as NCF or NCP.

亦可於半導體用接著劑中進一步調配離子阱、抗氧化劑、矽烷偶合劑、鈦偶合劑、調平劑等。該些可單獨使用一種,亦可組合使用兩種以上。關於該些調配量,只要適宜調整以顯現出各添加劑的效果即可。An ion trap, an antioxidant, a silane coupling agent, a titanium coupling agent, a leveling agent, etc. may also be further blended into the adhesive for semiconductors. These may be used individually by 1 type, and may be used in combination of 2 or more types. The blending amounts may be appropriately adjusted to express the effects of each additive.

本實施形態的半導體用接著劑可成形為膜狀。以下示出使用了本實施形態的半導體用接著劑的膜狀接著劑的製作方法的一例。The adhesive agent for semiconductors of this embodiment can be formed into a film shape. An example of a method for producing a film-like adhesive using the semiconductor adhesive of this embodiment is shown below.

首先,將(a)成分~(f)成分及添加劑中的必要成分添加至有機溶媒中,藉由攪拌混合、混煉等進行溶解或分散而製備樹脂清漆。其後,於實施了脫模處理的基材膜上,使用刮刀塗佈機、輥塗佈機、敷料器等來塗佈樹脂清漆後,藉由加熱而將有機溶媒去除,藉此可於基材膜上形成膜狀接著劑。First, necessary components among components (a) to (f) and additives are added to an organic solvent, and are dissolved or dispersed by stirring, mixing, kneading, etc. to prepare a resin varnish. Thereafter, the resin varnish is applied to the base film that has been subjected to the release treatment using a blade coater, a roll coater, an applicator, etc., and then the organic solvent is removed by heating, whereby the organic solvent can be applied to the base film. A film-like adhesive is formed on the material film.

膜狀接著劑的厚度並無特別限制,例如較佳為連接前的凸塊的高度的0.5倍~1.5倍,更佳為0.6倍~1.3倍,進而較佳為0.7倍~1.2倍。The thickness of the film adhesive is not particularly limited, but for example, it is preferably 0.5 to 1.5 times the height of the bump before connection, more preferably 0.6 to 1.3 times, and still more preferably 0.7 to 1.2 times.

若膜狀接著劑的厚度為凸塊的高度的0.5倍以上,則可充分抑制因未填充接著劑而引起的孔隙的產生,從而可進一步提高連接可靠性。另外,若厚度為1.5倍以下,則可充分抑制在連接時自晶片連接區域被擠出的接著劑的量,因此可充分防止接著劑向不必要的部分的附著。若膜狀接著劑的厚度大於1.5倍,則凸塊必須排除大量的接著劑,容易產生導通不良。另外,對於由窄間距化-多針腳化引起的凸塊的弱化(凸塊直徑的微小化)而言,排除大量的樹脂的情況會增大對凸塊的損傷,因此欠佳。If the thickness of the film-like adhesive is 0.5 times or more the height of the bump, the generation of voids caused by insufficient filling of the adhesive can be sufficiently suppressed, thereby further improving connection reliability. In addition, if the thickness is 1.5 times or less, the amount of adhesive extruded from the wafer connection area during connection can be sufficiently suppressed, and therefore adhesion of the adhesive to unnecessary parts can be sufficiently prevented. If the thickness of the film adhesive is greater than 1.5 times, a large amount of adhesive must be removed from the bump, which may easily cause poor conduction. In addition, regarding the weakening of the bumps (miniaturization of the bump diameter) caused by narrowing the pitch and increasing the number of pins, excluding a large amount of resin will increase damage to the bumps, which is not preferable.

通常凸塊的高度為5 μm~100 μm,據此,膜狀接著劑的厚度較佳為2.5 μm~150 μm,更佳為3.5 μm~120 μm。Generally, the height of the bumps is 5 μm to 100 μm. Accordingly, the thickness of the film adhesive is preferably 2.5 μm to 150 μm, and more preferably 3.5 μm to 120 μm.

作為樹脂清漆的製備中使用的有機溶媒,較佳為具有可使各成分均勻地溶解或分散的特性者,例如可列舉:二甲基甲醯胺、二甲基乙醯胺、N-甲基-2-吡咯啶酮、二甲基亞碸、二乙二醇二甲醚、甲苯、苯、二甲苯、甲基乙基酮、四氫呋喃、乙基溶纖劑、乙基溶纖劑乙酸酯、丁基溶纖劑、二噁烷、環己酮、及乙酸乙酯。該些有機溶媒可單獨使用或者組合使用兩種以上。製備樹脂清漆時的攪拌混合及混煉例如可使用攪拌機、磨碎機、三輥、球磨機、珠磨機或均質機來進行。The organic solvent used in the preparation of the resin varnish is preferably one that has the characteristics of uniformly dissolving or dispersing each component. Examples thereof include dimethylformamide, dimethylacetamide, and N-methyl. -2-pyrrolidinone, dimethylsyanin, diglyme, toluene, benzene, xylene, methyl ethyl ketone, tetrahydrofuran, ethyl cellosolve, ethyl cellosolve acetate , butyl cellosolve, dioxane, cyclohexanone, and ethyl acetate. These organic solvents can be used alone or in combination of two or more. Stirring, mixing, and kneading when preparing a resin varnish can be performed using a mixer, a grinder, a three-roller, a ball mill, a bead mill, or a homogenizer, for example.

作為基材膜,若為具有可耐受使有機溶媒揮發時的加熱條件的耐熱性者則並無特別限制,可例示:聚丙烯膜、聚甲基戊烯膜等聚烯烴膜;聚對苯二甲酸乙二酯膜、聚萘二甲酸乙二酯膜等聚酯膜;聚醯亞胺膜及聚醚醯亞胺膜。基材膜並不限定於包含該些膜的單層者,亦可為包含兩種以上的材料的多層膜。The base film is not particularly limited as long as it has heat resistance that can withstand the heating conditions for volatilizing the organic solvent. Examples include polyolefin films such as polypropylene films and polymethylpentene films; polyparaphenylene films. Polyester films such as ethylene dicarboxylate film and polyethylene naphthalate film; polyimide film and polyetherimide film. The base film is not limited to a single layer including these films, and may be a multilayer film including two or more materials.

使有機溶媒自塗佈於基材膜的樹脂清漆中揮發時的乾燥條件較佳設為有機溶媒充分揮發的條件,具體而言較佳為進行50℃~200℃、0.1分鐘~90分鐘的加熱。有機溶媒較佳為被去除至相對於膜狀接著劑總量而為1.5質量%以下。The drying conditions for volatilizing the organic solvent from the resin varnish applied to the base film are preferably conditions in which the organic solvent is fully volatilized. Specifically, it is preferable to perform heating at 50°C to 200°C for 0.1 to 90 minutes. . The organic solvent is preferably removed to 1.5% by mass or less relative to the total amount of the film adhesive.

另外,本實施形態的半導體用接著劑可直接形成於晶圓上。具體而言,例如可藉由將所述樹脂清漆直接旋塗於晶圓上而形成膜後將有機溶媒去除,而於晶圓上直接形成半導體用接著劑。In addition, the adhesive agent for semiconductors of this embodiment can be formed directly on a wafer. Specifically, for example, the resin varnish can be directly spin-coated on the wafer to form a film, and then the organic solvent can be removed to form the semiconductor adhesive directly on the wafer.

<半導體裝置> 對於本實施形態的半導體裝置,以下使用圖1及圖2來進行說明。圖1是表示本揭示的半導體裝置的一實施形態的示意剖面圖。如圖1的(a)所示,半導體裝置100具有:相互相向的半導體晶片10及基板(配線電路基板)20、分別配置於半導體晶片10及基板20的相互相向的面上的配線15、將半導體晶片10及基板20的配線15相互連接的連接凸塊30、以及無間隙地填充於半導體晶片10及基板20間的空隙中的接著材料40。半導體晶片10及基板20藉由配線15及連接凸塊30而經覆晶連接。配線15及連接凸塊30由接著材料40密封而與外部環境阻隔。<Semiconductor Device> The semiconductor device of this embodiment will be described below using FIGS. 1 and 2 . FIG. 1 is a schematic cross-sectional view showing an embodiment of the semiconductor device of the present disclosure. As shown in (a) of FIG. 1 , the semiconductor device 100 includes a semiconductor chip 10 and a substrate (wired circuit board) 20 facing each other, wiring 15 respectively arranged on the surfaces of the semiconductor chip 10 and the substrate 20 facing each other. The connection bumps 30 that connect the semiconductor wafer 10 and the wiring 15 of the substrate 20 to each other, and the adhesive material 40 that fills the gap between the semiconductor wafer 10 and the substrate 20 without any gap. The semiconductor chip 10 and the substrate 20 are flip-chip connected via wiring 15 and connection bumps 30 . The wiring 15 and the connection bump 30 are sealed by the adhesive material 40 and isolated from the external environment.

如圖1的(b)所示,半導體裝置200具有:相互相向的半導體晶片10及基板20、分別配置於半導體晶片10及基板20的相互相向的面上的凸塊32、以及無間隙地填充於半導體晶片10及基板20間的空隙中的接著材料40。半導體晶片10及基板20藉由相向的凸塊32相互連接而經覆晶連接。凸塊32由接著材料40密封而與外部環境阻隔。接著材料40為本實施形態的半導體用接著劑的硬化物。As shown in FIG. 1( b ), the semiconductor device 200 includes a semiconductor wafer 10 and a substrate 20 facing each other, bumps 32 respectively arranged on the mutually facing surfaces of the semiconductor wafer 10 and the substrate 20 , and a gap-free filling device. The adhesive material 40 is in the gap between the semiconductor chip 10 and the substrate 20 . The semiconductor chip 10 and the substrate 20 are connected to each other through opposite bumps 32 and are flip-chip connected. The bump 32 is sealed from the external environment by the adhesive material 40 . The subsequent material 40 is a cured product of the semiconductor adhesive of this embodiment.

圖2是表示本揭示的半導體裝置的另一實施形態的示意剖面圖。如圖2的(a)所示,半導體裝置300除了藉由配線15及連接凸塊30將兩個半導體晶片10覆晶連接的方面以外,與半導體裝置100相同。如圖2的(b)所示,半導體裝置400除了藉由凸塊32將兩個半導體晶片10覆晶連接的方面以外,與半導體裝置200相同。2 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present disclosure. As shown in FIG. 2( a ), the semiconductor device 300 is the same as the semiconductor device 100 except that two semiconductor chips 10 are flip-chip connected through the wiring 15 and the connection bump 30 . As shown in FIG. 2( b ), the semiconductor device 400 is the same as the semiconductor device 200 except that the two semiconductor chips 10 are flip-chip connected through the bumps 32 .

半導體晶片10並無特別限定,可使用由矽、鍺等同一種類的元素所構成的元素半導體;砷化鎵、磷化銦等化合物半導體。The semiconductor wafer 10 is not particularly limited, and may be an elemental semiconductor composed of one type of element such as silicon or germanium; or a compound semiconductor such as gallium arsenide or indium phosphide.

作為基板20,若為電路基板則並無特別限制,可使用:於以玻璃環氧、聚醯亞胺、聚酯、陶瓷、環氧、雙順丁烯二醯亞胺三嗪等作為主要成分的絕緣基板的表面上,將金屬膜的不需要的部位蝕刻去除而形成的具有配線(配線圖案)15的電路基板;於所述絕緣基板的表面藉由金屬鍍敷等而形成有配線15的電路基板;藉由於所述絕緣基板的表面上印刷導電性物質而形成有配線15的電路基板。As the substrate 20, if it is a circuit substrate, there is no particular limitation. It can use glass epoxy, polyimide, polyester, ceramic, epoxy, bismaleimide triazine, etc. as the main component. A circuit board with wiring (wiring pattern) 15 formed by etching and removing unnecessary parts of a metal film on the surface of an insulating substrate; and a circuit board with wiring 15 formed on the surface of the insulating substrate by metal plating or the like. Circuit board: a circuit board on which wiring 15 is formed by printing a conductive material on the surface of the insulating substrate.

配線15及凸塊32等連接部含有金、銀、銅、焊料(主成分例如為錫-銀、錫-鉛、錫-鉍、錫-銅、錫-銀-銅)、鎳、錫、鉛等作為主成分,亦可含有多種金屬。The connection parts such as the wiring 15 and the bump 32 contain gold, silver, copper, solder (the main component is, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, tin-silver-copper), nickel, tin, and lead etc. as the main component, and may also contain a variety of metals.

所述金屬中,就形成連接部的電傳導性-熱傳導性優異的封裝的觀點而言,較佳為金、銀及銅,更佳為銀及銅。就形成降低了成本的封裝的觀點而言,基於廉價而較佳為銀、銅及焊料,更佳為銅及焊料,進而較佳為焊料。若於室溫下於金屬的表面形成氧化膜,則存在生產性降低的情況及成本增加的情況,因此,就抑制氧化膜的形成的觀點而言,較佳為金、銀、銅及焊料,更佳為金、銀、焊料,進而較佳為金、銀。Among the above-mentioned metals, from the viewpoint of forming a package with excellent electrical conductivity and thermal conductivity of the connection portion, gold, silver, and copper are preferred, and silver and copper are more preferred. From the viewpoint of forming a cost-reduced package, silver, copper and solder are preferable due to low cost, copper and solder are more preferable, and solder is still more preferable. If an oxide film is formed on the surface of a metal at room temperature, productivity may decrease and costs may increase. Therefore, from the viewpoint of suppressing the formation of an oxide film, gold, silver, copper and solder are preferred. Gold, silver, and solder are more preferred, and gold and silver are even more preferred.

於所述配線15及凸塊32的表面上,亦可藉由例如鍍敷而形成有以金、銀、銅、焊料(主成分為例如錫-銀、錫-鉛、錫-鉍、錫-銅)、錫、鎳等作為主要成分的金屬層。該金屬層可僅包含單一的成分,亦可包含多種成分。另外,所述金屬層亦可呈單層或多個金屬層積層而成的結構。The surface of the wiring 15 and the bump 32 may also be formed with gold, silver, copper, solder (main components such as tin-silver, tin-lead, tin-bismuth, tin- Copper), tin, nickel and other metal layers as main components. The metal layer may contain only a single component or may contain multiple components. In addition, the metal layer may also have a structure in which a single layer or a plurality of metal layers are laminated.

圖1的(b)中,設置於半導體晶片10的表面的凸塊32亦可具有包括銅柱部與焊料部的多層結構。該情況下,較佳為銅柱部配置於半導體晶片10側,焊料部設置於銅柱部的端部。In FIG. 1( b ), the bump 32 provided on the surface of the semiconductor chip 10 may also have a multi-layer structure including a copper pillar part and a solder part. In this case, it is preferable that the copper pillar portion is disposed on the semiconductor chip 10 side, and the solder portion is provided at the end of the copper pillar portion.

另外,本實施形態的半導體裝置中,半導體裝置100~半導體裝置400中所示的結構(封裝)亦可積層有多個。該情況下,半導體裝置100~半導體裝置400亦可藉由包含金、銀、銅、焊料(主成分為例如錫-銀、錫-鉛、錫-鉍、錫-銅、錫-銀-銅)、錫、鎳等的凸塊或配線而相互電性連接。In addition, in the semiconductor device of this embodiment, a plurality of structures (packages) shown in the semiconductor device 100 to the semiconductor device 400 may be laminated. In this case, the semiconductor device 100 to the semiconductor device 400 may also be made of gold, silver, copper, and solder (the main components are, for example, tin-silver, tin-lead, tin-bismuth, tin-copper, and tin-silver-copper). , tin, nickel, etc. bumps or wiring to electrically connect each other.

作為將半導體裝置積層多個的方法,如圖3所示,例如可列舉TSV(Through-Silicon Via)技術。圖3是表示本揭示的半導體裝置的另一實施形態的示意剖面圖,且為使用TSV技術的半導體裝置。於圖3所示的半導體裝置500中,形成於中介層(interposer)50上的配線15經由連接凸塊30而與半導體晶片10的配線15連接,藉此將半導體晶片10與中介層50覆晶連接。於半導體晶片10與中介層50之間的空隙中無間隙地填充有接著材料40。於所述半導體晶片10中的與中介層50為相反側的表面上,經由配線15、連接凸塊30及接著材料40而反覆積層有半導體晶片10。半導體晶片10的表背的圖案面的配線15是藉由在貫穿半導體晶片10內部的孔內所填充的貫通電極34而相互連接。再者,作為貫通電極34的材質,可使用銅、鋁等。As a method of stacking a plurality of semiconductor devices, as shown in FIG. 3 , for example, TSV (Through-Silicon Via) technology can be used. 3 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present disclosure, and is a semiconductor device using TSV technology. In the semiconductor device 500 shown in FIG. 3 , the wiring 15 formed on the interposer 50 is connected to the wiring 15 of the semiconductor chip 10 through the connection bumps 30 , thereby flip-chip the semiconductor chip 10 and the interposer 50 connection. The gap between the semiconductor wafer 10 and the interposer 50 is filled with the adhesive material 40 without any gap. On the surface of the semiconductor wafer 10 opposite to the interposer 50 , the semiconductor wafer 10 is repeatedly laminated via the wiring 15 , the connection bump 30 and the adhesive material 40 . The wirings 15 on the pattern surfaces on the front and back of the semiconductor wafer 10 are connected to each other by through-electrodes 34 filled in holes penetrating the inside of the semiconductor wafer 10 . In addition, as the material of the through-electrode 34, copper, aluminum, etc. can be used.

藉由此種TSV技術,自通常不會使用的半導體晶片的背面亦可獲取訊號。進而,因於半導體晶片10內垂直地插通貫通電極34,故可縮短相向的半導體晶片10間、或者半導體晶片10及中介層50間的距離而進行柔軟的連接。於此種TSV技術中,本實施形態的半導體用接著劑可適用作相向的半導體晶片10間、或者半導體晶片10及中介層50間的半導體用接著劑。With this TSV technology, signals can be obtained from the backside of a semiconductor chip that is not normally used. Furthermore, since the through-electrodes 34 are vertically inserted into the semiconductor wafer 10 , the distance between the opposing semiconductor wafers 10 or between the semiconductor wafer 10 and the interposer 50 can be shortened to achieve a flexible connection. In such TSV technology, the semiconductor adhesive of this embodiment can be applied as a semiconductor adhesive between opposing semiconductor wafers 10 or between the semiconductor wafer 10 and the interposer 50 .

另外,於區域凸塊(area bump)晶片技術等自由度高的凸塊形成方法中,可不經由中介層而將半導體晶片直接封裝於母板(mother board)上。本實施形態的半導體用接著劑亦可適用於此種將半導體晶片直接封裝於母板上的情況。再者,於將兩個配線電路基板積層的情況下,將基板間的空隙密封時亦可適用本實施形態的半導體用接著劑。In addition, in a bump formation method with a high degree of freedom such as area bump wafer technology, the semiconductor chip can be directly packaged on a mother board without an interposer. The adhesive agent for semiconductors of this embodiment is also applicable to the case where a semiconductor chip is directly packaged on a motherboard. Furthermore, when two printed circuit boards are laminated, the adhesive agent for semiconductors of this embodiment can also be applied when sealing the gap between the board|substrates.

<半導體裝置的製造方法> 其次,對本實施形態的半導體裝置的製造方法進行說明。<Manufacturing method of semiconductor device> Next, a method for manufacturing a semiconductor device according to this embodiment will be described.

首先,在基板或半導體晶片上貼附膜狀接著劑。膜狀接著劑的貼附可藉由加熱壓製、輥層壓、真空層壓等來進行。膜狀接著劑的供給面積及厚度根據半導體晶片或基板的尺寸以及連接凸塊的高度適當設定。膜狀接著劑可貼附於半導體晶片上,亦可在貼附於半導體晶圓上後,藉由切割而單片化為半導體晶片,製作貼附有膜狀接著劑的半導體晶片。First, a film-like adhesive is attached to the substrate or semiconductor wafer. The film adhesive can be attached by heat pressing, roller lamination, vacuum lamination, etc. The supply area and thickness of the film-like adhesive are appropriately set according to the size of the semiconductor wafer or substrate and the height of the connection bump. The film adhesive can be attached to the semiconductor wafer, or it can be separated into semiconductor wafers by dicing after being attached to the semiconductor wafer, thereby producing a semiconductor wafer to which the film adhesive is attached.

於將膜狀接著劑貼附於基板或半導體晶片上後,使用覆晶接合機等連接裝置對半導體晶片的連接凸塊(焊料凸塊等)與基板的配線(銅配線等)進行對位。繼而,對半導體晶片與基板一邊以連接凸塊的熔點以上的溫度進行加熱一邊進行壓接,從而將半導體晶片與基板連接,並且藉由膜狀接著劑對半導體晶片與基板間的空隙進行密封填充。藉由以上所述而獲得半導體裝置。After the film-like adhesive is attached to the substrate or semiconductor wafer, a connection device such as a flip-chip bonding machine is used to align the connection bumps (solder bumps, etc.) of the semiconductor wafer with the wiring (copper wiring, etc.) of the substrate. Then, the semiconductor wafer and the substrate are pressure-bonded while being heated at a temperature above the melting point of the connection bumps, thereby connecting the semiconductor wafer and the substrate, and the gap between the semiconductor wafer and the substrate is sealed and filled with a film-like adhesive. . A semiconductor device is obtained as described above.

連接荷重可考慮連接凸塊的數量及高度的偏差、因加壓而產生的連接凸塊或承接連接部的凸塊的配線的變形量來設定。關於連接溫度,連接部的溫度較佳為連接凸塊的熔點以上,但只要為可形成各個連接部(凸塊或配線)的金屬接合的溫度即可。於連接凸塊為焊料凸塊的情況下,連接溫度亦可為約220℃以上。The connection load can be set taking into account variations in the number and height of the connection bumps, and the amount of deformation of the connection bumps or the wiring receiving the bumps in the connection portion due to pressurization. Regarding the connection temperature, the temperature of the connection portion is preferably not less than the melting point of the connection bump, but it may be a temperature at which metal bonding of each connection portion (bump or wiring) can be formed. When the connection bumps are solder bumps, the connection temperature can also be about 220°C or above.

連接時的連接時間根據連接部的構成金屬而不同,但就生產性提高的觀點而言,時間越短越佳。於連接凸塊為焊料凸塊的情況下,連接時間較佳為20秒以下,更佳為10秒以下,進而較佳為5秒以下。於使用焊料凸塊以短時間連接進行連接的情況下,連接時間較佳為4秒以下,更佳為3秒以下,進而較佳為2秒以下。藉由以所述方式在短時間內進行連接,可製造更多的高可靠性的封裝。此處,連接時間是指所述連接溫度花費在連接凸塊上的時間。於銅-銅或銅-金的金屬連接的情況下,連接時間較佳為60秒以下。於連接凸塊為焊料凸塊的情況下,較佳為在連接時使焊料熔融,去除氧化膜及表面的雜質,在連接部形成金屬接合。The connection time during connection varies depending on the constituent metal of the connection part, but from the viewpoint of improving productivity, the shorter the time, the better. When the connection bumps are solder bumps, the connection time is preferably 20 seconds or less, more preferably 10 seconds or less, and still more preferably 5 seconds or less. In the case of short-time connection using solder bumps, the connection time is preferably 4 seconds or less, more preferably 3 seconds or less, and still more preferably 2 seconds or less. By making connections in a short time in this manner, more high-reliability packages can be manufactured. Here, the connection time refers to the time the connection temperature takes to reach the connection bump. In the case of copper-copper or copper-gold metal connection, the connection time is preferably 60 seconds or less. When the connection bumps are solder bumps, it is preferable to melt the solder during connection to remove the oxide film and surface impurities to form a metal joint at the connection portion.

於本實施形態的半導體裝置的製造方法中,亦可於對位後進行暫時固定(介隔有半導體用接著劑的狀態),並利用回焊爐進行加熱處理,藉此使連接凸塊熔融而將半導體晶片與基板連接。因於暫時固定的階段中並非必須形成金屬接合,故與所述一邊進行加熱一邊進行壓接的方法相比,可進行低荷重、短時間、低溫度下的壓接,生產性提高,並且可抑制連接部的劣化。In the method of manufacturing a semiconductor device according to this embodiment, the connection bumps may be melted by temporarily fixing (with a semiconductor adhesive interposed therebetween) after alignment and performing heat treatment in a reflow furnace. Connect the semiconductor wafer to the substrate. Since it is not necessary to form a metal joint in the temporary fixation stage, compared with the above-mentioned method of performing pressure bonding while heating, pressure bonding can be performed with a low load, a short time, and a low temperature, thereby improving productivity and enabling Suppresses deterioration of connection parts.

另外,亦可於將半導體晶片與基板連接後利用烘箱等進行加熱處理,從而進一步提高連接可靠性-絕緣可靠性。加熱溫度較佳為膜狀接著劑進行硬化的溫度,更佳為完全硬化的溫度。加熱溫度、加熱時間可適當設定。In addition, after the semiconductor chip is connected to the substrate, heat treatment may be performed using an oven or the like, thereby further improving connection reliability and insulation reliability. The heating temperature is preferably a temperature at which the film-like adhesive is hardened, and more preferably a temperature at which it is completely hardened. The heating temperature and heating time can be set appropriately.

本實施形態的半導體裝置的製造方法中,亦可於基板或半導體晶片上供給糊狀的半導體用接著劑來代替膜狀接著劑。半導體用接著劑的供給可藉由旋塗等塗佈方法進行。In the method of manufacturing a semiconductor device according to this embodiment, a paste-like semiconductor adhesive may be supplied on the substrate or semiconductor wafer instead of the film-like adhesive. The adhesive for semiconductors can be supplied by a coating method such as spin coating.

以上,對本揭示的適宜的實施形態進行了說明,但本揭示並不限定於所述實施形態。 [實施例]The preferred embodiments of the present disclosure have been described above, but the present disclosure is not limited to the embodiments. [Example]

以下,藉由實施例來更具體地說明本揭示,但本揭示並不限定於實施例。Hereinafter, the present disclosure will be explained in more detail using examples, but the present disclosure is not limited to the examples.

各實施例及比較例中使用的化合物如下所述。 (a)成分:重量平均分子量小於10000的樹脂 (a-1):含三苯酚甲烷骨架的多官能環氧樹脂(三菱化學股份有限公司製造,商品名「EP1032H60」,重量平均分子量:800~2000) (a-2):雙酚F型液狀環氧樹脂(三菱化學股份有限公司製造,商品名「YL983U」,重量平均分子量:約340) (a-3):可撓性半固體狀環氧樹脂(三菱化學股份有限公司製造,商品名「YX7110B60」,重量平均分子量:約1000~5000)The compounds used in each Example and Comparative Example are as follows. (a) Ingredient: Resin with weight average molecular weight less than 10,000 (a-1): Multifunctional epoxy resin containing trisphenolmethane skeleton (manufactured by Mitsubishi Chemical Co., Ltd., trade name "EP1032H60", weight average molecular weight: 800 to 2000) (a-2): Bisphenol F-type liquid epoxy resin (manufactured by Mitsubishi Chemical Co., Ltd., trade name "YL983U", weight average molecular weight: approximately 340) (a-3): Flexible semi-solid epoxy resin (manufactured by Mitsubishi Chemical Co., Ltd., trade name "YX7110B60", weight average molecular weight: about 1000 to 5000)

(b)成分:硬化劑:2,4-二胺基-6-[2'-甲基咪唑-(1')]-乙基-均三嗪異三聚氰酸加成物(四國化成股份有限公司製造,商品名「2MAOK-PW」)(b) Ingredients: Hardener: 2,4-diamino-6-[2'-methylimidazole-(1')]-ethyl-s-triazine isocyanuric acid adduct (manufactured by Shikoku Chemical Co., Ltd., trade name "2MAOK-PW")

(c)成分:重量平均分子量為10000以上的高分子化合物:苯氧基樹脂(東都化成股份有限公司製造,商品名「ZX1356」,Tg:約71℃,重量平均分子量:約63000)(c) Ingredients: Polymer compound with a weight average molecular weight of 10,000 or more: Phenoxy resin (manufactured by Toto Chemical Co., Ltd., trade name "ZX1356", Tg: about 71°C, weight average molecular weight: about 63,000)

(d)成分:助熔劑(羧酸):戊二酸(熔點:約95℃)(d) Ingredients: Flux (carboxylic acid): glutaric acid (melting point: about 95°C)

(e)成分:無機填料 (e-1)二氧化矽填料(亞都瑪科技(Admatechs)股份有限公司製造,商品名「SE2050」,平均粒徑:0.5 μm) (e-2)甲基丙烯酸表面處理奈米二氧化矽填料(亞都瑪科技(Admatechs)股份有限公司製造,商品名「YA050C-SM」,平均粒徑:約50 nm)(e) Ingredients: Inorganic filler (e-1) Silica filler (manufactured by Admatechs Co., Ltd., trade name "SE2050", average particle size: 0.5 μm) (e-2) Methacrylic surface-treated nanosilica filler (manufactured by Admatechs Co., Ltd., trade name "YA050C-SM", average particle size: about 50 nm)

(f)成分:有機填料 (f-1):矽酮複合粉末(信越化學工業股份有限公司製造,商品名「KMP-602」,平均粒徑:30 μm,球狀矽酮橡膠粉末的表面經矽酮樹脂被覆的球狀粉末) (f-2):矽酮複合粉末(信越化學工業股份有限公司製造,商品名「KMP-600」,平均粒徑:5 μm,球狀矽酮橡膠粉末的表面經矽酮樹脂被覆的球狀粉末) (f-3):矽酮複合粉末(信越化學工業股份有限公司製造,商品名「KMP-605」,平均粒徑:2 μm,球狀矽酮橡膠粉末的表面經矽酮樹脂被覆的球狀粉末) (f-4):矽酮複合粉末(信越化學工業股份有限公司製造,商品名「X-52-7030」,平均粒徑:0.8 μm,球狀矽酮橡膠粉末的表面經矽酮樹脂被覆的球狀粉末) (f-5):核殼型有機微粒子(日本羅門哈斯(Rohm and Haas Japan)股份有限公司製造,商品名「EXL-2655」,核部分:丁二烯/苯乙烯共聚聚合物,殼部分:PMMA/苯乙烯共聚聚合物)(f) Ingredients: organic fillers (f-1): Silicone composite powder (manufactured by Shin-Etsu Chemical Industry Co., Ltd., trade name "KMP-602", average particle diameter: 30 μm, spherical silicone rubber powder whose surface is coated with silicone resin) powder) (f-2): Silicone composite powder (manufactured by Shin-Etsu Chemical Industry Co., Ltd., trade name "KMP-600", average particle diameter: 5 μm, spherical silicone rubber powder whose surface is coated with silicone resin) powder) (f-3): Silicone composite powder (manufactured by Shin-Etsu Chemical Industry Co., Ltd., trade name "KMP-605", average particle diameter: 2 μm, spherical silicone rubber powder whose surface is coated with silicone resin) powder) (f-4): Silicone composite powder (manufactured by Shin-Etsu Chemical Industry Co., Ltd., trade name "X-52-7030", average particle diameter: 0.8 μm, spherical silicone rubber powder whose surface is coated with silicone resin spherical powder) (f-5): Core-shell type organic fine particles (manufactured by Rohm and Haas Japan Co., Ltd., trade name "EXL-2655", core part: butadiene/styrene copolymer, shell part : PMMA/styrene copolymer)

(實施例1~實施例4及比較例1~比較例2) <膜狀接著劑的製作> 將表1所示的調配量(單位:質量份)的(a)成分、(b)成分、(c)成分、(d)成分、(e)成分及(f)成分以NV值([乾燥後的塗料成分質量]/[乾燥前的塗料成分質量]×100)成為60質量%的方式添加於有機溶媒(甲基乙基酮)中。其後,添加與所述(a)成分~(f)成分及有機溶媒的總調配量相同質量的ϕ1.0 mm的二氧化鋯珠粒,利用球磨機(日本弗里茨(Fritsch Japan)股份有限公司製造,行星式微粉碎機P-7)攪拌30分鐘。於攪拌後藉由過濾而去除二氧化鋯珠粒,從而製作塗敷清漆。(Example 1 to Example 4 and Comparative Example 1 to Comparative Example 2) <Preparation of film adhesive> The (a) component, (b) component, (c) component, (d) component, (e) component, and (f) component were prepared in the preparation amounts (unit: parts by mass) shown in Table 1 and calculated as the NV value ([dry It is added to the organic solvent (methyl ethyl ketone) so that the mass of the paint component after drying/[the mass of the paint component before drying] × 100) becomes 60 mass %. Thereafter, zirconium dioxide beads having the same mass of ϕ1.0 mm as the total amount of components (a) to (f) and the organic solvent were added, and the mixture was milled using a ball mill (Fritsch Japan Co., Ltd. Manufactured by the company, planetary micro-pulverizer P-7) stir for 30 minutes. After stirring, the zirconium dioxide beads are removed by filtration to produce a coating varnish.

利用台式塗佈機(平野金屬(HIRANO KINZOKU)公司製造)塗敷所得的塗敷清漆,於80℃下乾燥5分鐘,藉此獲得膜厚20 μm的膜狀接著劑。The obtained coating varnish was applied with a desktop coater (manufactured by HIRANO KINZOKU Co., Ltd.) and dried at 80° C. for 5 minutes to obtain a film-like adhesive with a film thickness of 20 μm.

利用以下所示的評價方法評價實施例及比較例中所得的膜狀接著劑的接著力及可靠性、以及使用其製作的半導體裝置的翹曲。評價結果如表1所示。The following evaluation methods were used to evaluate the adhesive strength and reliability of the film adhesives obtained in the Examples and Comparative Examples, and the warpage of the semiconductor devices produced using them. The evaluation results are shown in Table 1.

<接著力的測定> 將膜狀接著劑剪切成既定的尺寸(縱3.2 mm×橫3.2 mm×厚度0.02 mm),於70℃下貼附至矽晶片(縱3 mm×橫3 mm×厚度0.725 mm)上,使用熱壓接試驗機(日立化成電子工廠股份有限公司製造),壓接(壓接條件:於壓接頭溫度190℃下壓接5秒後,於壓接頭溫度240℃下壓接5秒,荷重0.5 MPa)至另一矽晶片(縱5 mm×橫5 mm×厚度0.725 mm)。其後,於潔淨烘箱(愛斯佩克(ESPEC)公司製造)中,進行硬化(175℃,2小時),從而獲得試驗樣品。<Measurement of adhesive force> Cut the film adhesive into a predetermined size (length 3.2 mm × width 3.2 mm × thickness 0.02 mm), attach it to the silicon wafer (length 3 mm × width 3 mm × thickness 0.725 mm) at 70°C, and use Thermocompression bonding testing machine (manufactured by Hitachi Chemical Electronics Factory Co., Ltd.), crimping (crimping conditions: crimping for 5 seconds at a crimping head temperature of 190°C, then crimping for 5 seconds at a crimping head temperature of 240°C, load 0.5 MPa) to another silicon wafer (length 5 mm × width 5 mm × thickness 0.725 mm). Thereafter, hardening (175° C., 2 hours) was performed in a clean oven (manufactured by ESPEC Co., Ltd.) to obtain a test sample.

將所述試驗樣品於85℃、相對濕度85%的恆溫恆濕槽(愛斯佩克(ESPEC)公司製造)內放置24小時,並在取出後,於250℃的加熱板上使用接著力測定裝置(達歌(DAGE)公司製造),於距下側的矽晶片的上表面的工具高度0.05 mm、工具速度0.05 mm/s的條件下測定接著力(吸濕後的250℃下的接著力)。The test sample was placed in a constant temperature and humidity chamber (manufactured by ESPEC) at 85°C and 85% relative humidity for 24 hours, and after being taken out, the adhesion force was measured on a hot plate at 250°C. The device (manufactured by DAGE) measures the adhesion force (adhesion force at 250°C after moisture absorption) at a tool height of 0.05 mm from the upper surface of the lower silicon wafer and a tool speed of 0.05 mm/s. ).

<耐回焊性的評價> 將膜狀接著劑剪切成既定的尺寸(縱7.3 mm×橫7.3 mm×厚度0.04 mm),貼附至帶焊料凸塊的半導體晶片(晶片尺寸:縱7.3 mm×橫7.3 mm×厚度0.15 mm,連接部的金屬:銅柱+焊料、凸塊高度(銅柱+焊料的合計高度):約45 μm)的凸塊側的面上,利用覆晶安裝裝置「FCB3」安裝(安裝條件:於以100℃/0.5 MPa/1 s暫時壓接後,升溫至180℃/0.5 MPa/2 s,其後於260℃/0.5 MPa/5 s的條件下進行正式壓接)在玻璃環氧基板(玻璃環氧基材的厚度:0.42 mm、銅配線的厚度:9 μm)上,獲得半導體裝置。膜狀接著劑藉由積層兩片膜厚20 μm者而使膜厚為40 μm。壓接時放置基板的載物台溫度為80℃。使用密封材料(日立化成股份有限公司製造,商品名「CEL9750ZHF10」),於180℃、6.75 MPa、90秒的條件下成型所述半導體裝置,於潔淨烘箱(愛斯佩克(ESPEC)公司製造)中,進行硬化(175℃,2小時),從而獲得試驗樣品。<Evaluation of reflow resistance> The film adhesive was cut into a predetermined size (7.3 mm in height × 7.3 mm in width × 0.04 mm in thickness), attached to the bump side of a semiconductor chip with solder bumps (chip size: 7.3 mm in height × 7.3 mm in width × 0.15 mm in thickness, metal of the connection part: copper pillar + solder, bump height (total height of copper pillar + solder): about 45 μm), and mounted using the flip chip mounting device "FCB3" (mounting conditions: after temporary compression bonding at 100℃/0.5 MPa/1 s, the temperature was raised to 180℃/0.5 MPa/2 s, and then at 260℃/0.5 MPa/5 s) on a glass epoxy substrate (thickness of the glass epoxy substrate: 0.42 mm, thickness of the copper wiring: 9 μm) to obtain a semiconductor device. The film adhesive was made 40 μm thick by laminating two sheets of 20 μm thick film. The stage temperature on which the substrate was placed during the press bonding was 80°C. Using a sealing material (manufactured by Hitachi Chemical Co., Ltd., trade name "CEL9750ZHF10"), the semiconductor device was molded under the conditions of 180°C, 6.75 MPa, and 90 seconds, and hardened (175°C, 2 hours) in a clean oven (manufactured by ESPEC) to obtain a test sample.

其次,於電子裝置工程聯合委員會(Joint Electron Device Engineering Council,JEDEC)水準2的條件下處理所述試驗樣品後,使其通過3次(最高到達溫度260℃)回焊爐(田村製作所股份有限公司製造)。使用萬用錶(科斯特(CUSTOM)公司製造)測定回焊前後的封裝的連接電阻值。將回焊前後的連接電阻值的變化量為5 Ω以下的情況作為評價「A」,將變化量超過5 Ω或者連接不良的情況作為評價「B」。Next, after processing the test sample under the conditions of Joint Electron Device Engineering Council (JEDEC) Level 2, it was passed through a reflow furnace (Tamura Manufacturing Co., Ltd., with a maximum temperature of 260°C) three times. manufacturing). Use a multimeter (manufactured by CUSTOM) to measure the connection resistance value of the package before and after reflow soldering. When the change in the connection resistance value before and after reflow is 5 Ω or less, the evaluation is "A", and when the change exceeds 5 Ω or the connection is poor, the evaluation is "B".

<翹曲評價> 利用與耐回焊性的評價相同的方法製作半導體裝置,並將其作為試驗樣品。對於所述試驗樣品,使用非接觸式形狀測定裝置(索尼(SONY)公司製造),測量從上方觀察晶片時的對角方向的兩邊的形狀。將各邊的凹凸的最大值與最小值的差作為翹曲量(μm),利用兩邊的平均值評價翹曲量。將該翹曲量為70 μm以下的情況作為評價「A」,將超過70 μm的情況作為評價「B」。<Warp evaluation> A semiconductor device was produced using the same method as for the evaluation of reflow resistance and used as a test sample. For the test sample, a non-contact shape measuring device (manufactured by Sony Corporation) was used to measure the shape of both sides in the diagonal direction when the wafer was viewed from above. The difference between the maximum value and the minimum value of the unevenness on each side was defined as the amount of warpage (μm), and the amount of warpage was evaluated using the average value of both sides. The case where the amount of warpage is 70 μm or less is evaluated as "A", and the case where the amount of warpage exceeds 70 μm is evaluated as "B".

[表1]   實施例 比較例 1 2 3 4 1 2 (a)成分 (a-1) 45 45 45 45 45 45 (a-2) 15 15 15 15 15 15 (a-3) 5 5 5 5 5 5 (b)成分 2 2 2 2 2 2 (c)成分 30 30 30 30 30 30 (d)成分 4 4 4 4 4 4 (e)成分 (e-1) 30 30 30 30 30 - (e-2) 45 45 45 45 45 - (f)成分 (f-1) 10 - - - - - (f-2) - 10 - - - - (f-3) - - 10 - - - (f-4) - - - 10 - - (f-5) - - - - 10 85 接著力(MPa) 10 10 10 9 10 3 耐回焊性 A A A A A B 翹曲 A A A A B A [Table 1] Embodiment Comparison Example 1 2 3 4 1 2 (a) Ingredients (a-1) 45 45 45 45 45 45 (a-2) 15 15 15 15 15 15 (a-3) 5 5 5 5 5 5 (b) Ingredients 2 2 2 2 2 2 (c) Ingredients 30 30 30 30 30 30 (d) Ingredients 4 4 4 4 4 4 (e) Ingredients (e-1) 30 30 30 30 30 - (e-2) 45 45 45 45 45 - (f) Ingredients (f-1) 10 - - - - - (f-2) - 10 - - - - (f-3) - - 10 - - - (f-4) - - - 10 - - (f-5) - - - - 10 85 Adhesion force (MPa) 10 10 10 9 10 3 Reflow resistance A A A A A B Curve A A A A B A

根據表1所示的結果明確般,確認到含有無機填料及矽酮橡膠填料的實施例1~實施例4的半導體用接著劑與比較例1~比較例2的半導體用接著劑相比,接著力及耐回焊性優異,且可實現低翹曲化。From the results shown in Table 1, it was clearly confirmed that the adhesives for semiconductors of Examples 1 to 4 containing inorganic fillers and silicone rubber fillers were more adhesive than the adhesives for semiconductors of Comparative Examples 1 to 2. It has excellent strength and reflow resistance and can achieve low warpage.

10:半導體晶片 15:配線(連接部) 20:基板(配線電路基板) 30:連接凸塊 32:凸塊(連接部) 34:貫通電極 40:接著材料 50:中介層 100、200、300、400、500:半導體裝置10:Semiconductor wafer 15: Wiring (connection part) 20:Substrate (wiring circuit board) 30:Connection bumps 32: Bump (connection part) 34:Through electrode 40:Add materials 50:Intermediate layer 100, 200, 300, 400, 500: semiconductor device

圖1是表示本揭示的半導體裝置的一實施形態的示意剖面圖。 圖2是表示本揭示的半導體裝置的另一實施形態的示意剖面圖。 圖3是表示本揭示的半導體裝置的另一實施形態的示意剖面圖。FIG. 1 is a schematic cross-sectional view showing an embodiment of the semiconductor device of the present disclosure. 2 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present disclosure. 3 is a schematic cross-sectional view showing another embodiment of the semiconductor device of the present disclosure.

10:半導體晶片 10:Semiconductor wafer

15:配線(連接部) 15: Wiring (connection part)

20:基板(配線電路基板) 20:Substrate (wiring circuit board)

30:連接凸塊 30:Connection bumps

32:凸塊(連接部) 32: Bump (connection part)

40:接著材料 40:Add materials

100、200:半導體裝置 100, 200: Semiconductor devices

Claims (9)

一種半導體用接著劑,含有重量平均分子量小於10000的樹脂、硬化劑、無機填料及矽酮橡膠填料,其中以半導體用接著劑的固體成分總量為基準,所述重量平均分子量小於10000的樹脂的含量為5質量%~75質量%,所述無機填料的含量為20質量%~50質量%,所述矽酮橡膠填料的含量為0.1質量%~20質量%。 An adhesive for semiconductors, containing a resin with a weight average molecular weight of less than 10,000, a hardener, an inorganic filler and a silicone rubber filler, wherein based on the total solid content of the adhesive for semiconductors, the resin with a weight average molecular weight of less than 10,000 The content is 5% to 75% by mass, the content of the inorganic filler is 20% to 50% by mass, and the content of the silicone rubber filler is 0.1% to 20% by mass. 如請求項1所述的半導體用接著劑,其中所述矽酮橡膠填料的平均粒徑為30μm以下。 The adhesive for semiconductors according to claim 1, wherein the silicone rubber filler has an average particle size of 30 μm or less. 如請求項1或2所述的半導體用接著劑,其中所述無機填料含有二氧化矽填料。 The adhesive for semiconductors according to claim 1 or 2, wherein the inorganic filler contains a silica filler. 如請求項1或2所述的半導體用接著劑,進一步含有重量平均分子量為10000以上的高分子成分。 The adhesive for semiconductors according to claim 1 or 2 further contains a polymer component having a weight average molecular weight of 10,000 or more. 如請求項4所述的半導體用接著劑,其中所述高分子成分的重量平均分子量為30000以上,所述高分子成分的玻璃轉移溫度為100℃以下。 The adhesive for semiconductors according to claim 4, wherein the weight average molecular weight of the polymer component is 30,000 or more, and the glass transition temperature of the polymer component is 100°C or less. 如請求項1或2所述的半導體用接著劑,為膜狀。 The adhesive for semiconductors according to claim 1 or 2 is in a film form. 如請求項1或2所述的半導體用接著劑,其中所述矽酮橡膠填料的含量相對於所述無機填料的含量的質量比為0.05~0.5。 The adhesive for semiconductors according to claim 1 or 2, wherein the mass ratio of the content of the silicone rubber filler to the content of the inorganic filler is 0.05 to 0.5. 一種半導體裝置的製造方法,為製造半導體晶片及配 線電路基板各自的連接部相互電性連接的半導體裝置、或者多個半導體晶片各自的連接部相互電性連接的半導體裝置的方法,所述半導體裝置的製造方法包括:使用如請求項1至7中任一項所述的半導體用接著劑對所述連接部的至少一部分進行密封的步驟。 A method of manufacturing a semiconductor device, which is to manufacture semiconductor wafers and components A method of manufacturing a semiconductor device in which connecting portions of line circuit substrates are electrically connected to each other, or a semiconductor device in which connecting portions of a plurality of semiconductor wafers are electrically connected to each other. The method of manufacturing the semiconductor device includes: using the method of claims 1 to 7 The step of sealing at least part of the connection portion with the semiconductor adhesive according to any one of the above. 一種半導體裝置,包括:由半導體晶片及配線電路基板各自的連接部相互電性連接而成的連接結構、或者由多個半導體晶片各自的連接部相互電性連接而成的連接結構;以及將所述連接部的至少一部分密封的接著材料,所述接著材料包含如請求項1至7中任一項所述的半導體用接著劑的硬化物。 A semiconductor device including: a connection structure in which connection portions of a semiconductor chip and a printed circuit board are electrically connected to each other, or a connection structure in which connection portions of a plurality of semiconductor wafers are electrically connected to each other; and An adhesive material for sealing at least part of the connection portion, the adhesive material including a cured product of the semiconductor adhesive according to any one of claims 1 to 7.
TW109110054A 2019-03-26 2020-03-25 Adhesive for semiconductors, manufacturing method of semiconductor device, and semiconductor device TWI834852B (en)