JPS583754A - Preventing method for thermal fatigue in meniscus part of mold for continuous casting - Google Patents

Preventing method for thermal fatigue in meniscus part of mold for continuous casting

Info

Publication number
JPS583754A
JPS583754A JP10367181A JP10367181A JPS583754A JP S583754 A JPS583754 A JP S583754A JP 10367181 A JP10367181 A JP 10367181A JP 10367181 A JP10367181 A JP 10367181A JP S583754 A JPS583754 A JP S583754A
Authority
JP
Japan
Prior art keywords
parts
mold
bolts
molds
thermal fatigue
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP10367181A
Other languages
Japanese (ja)
Inventor
Akira Kubota
昭 久保田
Yasuhiko Kinoshita
康彦 木下
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mishima Kosan Co Ltd
Original Assignee
Mishima Kosan Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mishima Kosan Co Ltd filed Critical Mishima Kosan Co Ltd
Priority to JP10367181A priority Critical patent/JPS583754A/en
Publication of JPS583754A publication Critical patent/JPS583754A/en
Pending legal-status Critical Current

Abstract

PURPOSE:To prevent the cracking of mold bodies owing to their thermal fatigue and to extend the life of the molds in the stage of connecting the mold bodies and back frames by means of lock bolts by fitting the tie bolts loosely into bolt insertion holes. CONSTITUTION:When molten steel of high temps. contacts with the inside surface of the long side parts 2 of molds, the long side parts (more particularly, meniscus parts) of the molds expand. When the inside surfaces of the parts 2 are cooled by the drop of the level of the molten steel coupled by the effect of cooling with cooling water, said parts shrink. Since tie bolts 5 fixing back frames 1 and the mold bodies 2 are fitted loosely in insertion holes for tie bolts, the expansion and contraction of the parts 2 in accordance with their heating and cooling are not restricted at all and the bolts 5 are fixed to have no looseness only in their axial line direction by the elastic forces of belleville springs 9.

Description

【発明の詳細な説明】 零発@確連続鋳造層鋳型のメニスカス部の熱疲労W止2
F法に関するものである。
[Detailed description of the invention] Thermal fatigue W prevention of meniscus part of zero-start @ reliable continuous casting layer mold 2
This is related to the F method.

−穀に連続鋳造装置Wは1III製鋳瓢本体を、骨の背
面から#I製のパックフレームで支持した様な形式のも
のであり、−蓋本体とパックフレームとは多数の鋳付ポ
ルトで強−に締結されcV%る。その為に操業中に一鯛
により鋳飄本体が加熱され11111シようとしてもパ
ックフレー^に拘束され自由lI!形が出来ず層性**
を起こす結果となる。そのS溶嗣湯田が低下し上記ma
w形した部分が冷却されるとl11部所に棹組1lIF
6カが働(事となる。以上の様な挙動が繰返されて1%
る中に鋳型内面メニスカス部が疲労しal1部所にクラ
ックが発生し、鋳型の寿命を短くする。
- Continuous casting device W is of a type in which a 1III cast gourd body is supported by a #I pack frame from the back of the bone, - The lid body and pack frame are formed by numerous casting ports. It is strongly connected to cV%. Therefore, during operation, the main body of the cast iron is heated by the sea bream, and even if you try to do it, it will be restrained by the pack flame and you will be free! Unable to form and layered**
This results in the occurrence of That S Totsugu Yuda lowered the above ma
When the w-shaped part is cooled, the neck is placed in the 11 part.
6 forces work (this happens. The above behavior is repeated and 1%
During this process, the inner meniscus of the mold becomes fatigued and cracks occur at the Al1 portion, shortening the life of the mold.

本発明1よ上述の欠点を解消する方法に係り、その要w
確、パックフレームと鋳匿本体とを締付ポルトで連結す
るに際し、締付ボルト顕部とパックフレーム間にOリン
グ4!耘装したOリングホルダー及び皿バネを介在さ曽
、しかも鋳付ボルトを11締付ボルト速通孔に遊嵌状に
ならしめたことを時機とする連続鋳造用鋳型メニスカス
部熱疲労肪止方法である。
The present invention 1 relates to a method for solving the above-mentioned drawbacks, and its main points w
When connecting the pack frame and the casting body with the tightening port, there must be an O-ring 4 between the tightening bolt part and the pack frame! A method for fixing fat due to thermal fatigue at the meniscus of a mold for continuous casting by using a fitted O-ring holder and a disc spring, and also by loosely fitting a casting bolt into a quick-through hole for a 11-tightening bolt. It is.

以下−mを参〜9しながら本原発一方9:壱群逃する。While referring to -m to 9 below, this nuclear power plant, on the other hand, 9: 1 group missed.

111図は連続鋳造装置の用Snx圓であり、(1)建
パックフレーム、(3)ば鯛もしくは鯛壷金憶の鋳臘本
体長w都、(3)は同値辺部であり、短辺部線長g11
薄櫓内側に靭込まれて詐る。(4) 、(4)・・・・
・・け曽付ボルト轡遥孔である。第2図は、上記した鋳
型の長if部とパックフレームとを締付ボルト(箒)に
て、一定する一実篇例をボしたものであり、(6)はパ
ックフレーム内部に設けられた冷却水S通溝である。(
7)はOリング、(1)goリング傘ルダー、(1)は
ニパネであり、譲ユパネは外側を高(曽しめて、Ill
!に力を付与曽しめc7動る。また第sew健、鋳型の
熱疲労防止機構の他の実罵倒を示すものであり、(10
)はパックフレームとOリング傘ルダーとの聞に命II
薯曽る鯛パツキンである。
Figure 111 shows the Snx circle for continuous casting equipment, (1) the Ken-pack frame, (3) the length of the body of the casting body of the sea bream or the sea bream pot Kinmei, (3) is the equivalence side, and the short side is Department line length g11
It is hidden inside the thin turret. (4) , (4)...
...This is a far hole for the bolt. Figure 2 shows an actual example in which the long if part of the mold described above and the pack frame are fixed with a tightening bolt (broom), and (6) is a bolt installed inside the pack frame. This is the cooling water S channel. (
7) is an O-ring, (1) is a go-ring umbrella rudder, (1) is a Nipane, and the Yupane has a high outer side.
! Gives power to c7 and moves. In addition, it shows other actual criticisms of the thermal fatigue prevention mechanism of the mold, (10
) is the life between the pack frame and O-ring umbrella rule.
This is a sea bream patsukin.

以上のようなamに係る本願発明によれば、高温の慴鯛
が鋳型の長辺部8爾に接触す番と、鋳国長辺舊(待にメ
ニスカス部)建、第1Wi中ム矢厭方向grimする0
次−′e−鯛のレベルが低下し、1kIIIJ水による
冷部の作用も槓作うて鋳麿長辺部内面が1に却されると
、第1図中B矢示方向に取aする。すなわち、本願発明
方法では、パックフレームと鋳型本体とをII窯して一
墨鋳付ボルトが、締付ボルト神道孔に遊嵌状に取付け−
hlzWゞ・52“0加熱1“5”4511II取lI
建、何ら馬制されることな(、シ無も締付ボルトは、ニ
パネの弾性力によりその軸線方向につ−ての緩みがな−
ように固定される。モしてOりング及び又はパツキンの
働きにより1冷却水が締付ボルト神通孔を過Vて震れる
こと4堕止してhる。
According to the present invention related to am as described above, when the high temperature sea bream comes into contact with the long side part 8 of the mold, when the long side of the casting country (the meniscus part) is fixed, and when the first Wi direction grim0
Next -'e- When the level of the sea bream decreases, and the inner surface of the long side of the cast mackerel is reduced to 1 due to the action of the cooling part by 1kIIIJ water, the sea bream is taken in the direction of the arrow B in Figure 1. . That is, in the method of the present invention, the pack frame and the mold body are heated in a II kiln, and the Isumi casting bolt is loosely fitted into the tightening bolt Shinto hole.
hlzWゞ・52"0 heating 1"5"4511II
The tightening bolt will not be loosened in the axial direction due to the elastic force of the clamp.
It will be fixed like this. Due to the action of the O-ring and/or packing, 1) the cooling water passes through the hole of the tightening bolt and vibrates; 4) it stops.

又、184図は締付ボルト神道孔をパックフレームの中
心部から両外側に向かって次第に長(、中心を偏心させ
た長孔状となし社W式の物の説maiであり、この第4
WJに示T型式の物によれば、鋳型長辺部の膨彊坂縮に
よる変位量が、胃外側に杼(につれて大となることに起
園する不備をも解消することができる。
In addition, Figure 184 shows the tightening bolt Shinto hole gradually lengthening from the center of the pack frame toward both outside sides (this is a long hole shape with the center eccentric), and this fourth
According to the T-type product shown in WJ, it is possible to solve the problem that the displacement amount due to expansion and contraction of the long side of the mold becomes larger as the size increases as the size increases as the size of the shaft increases as the size increases as the size of the shaft increases.

以上述べてきたように、本願発晒方II!によれば、一
層長辺部の加熱冷却に伴なう膨鵬坂細が自由に行ない得
るので、鋳型本体の−aSによる−れを防止でき、鋳型
の寿命を長くすることがで會る。×、足バネにより締付
力を一定Iz鳩節することがで會るので、−付方の管理
を正確に行なうことがで會る。
As mentioned above, how to expose the original application II! According to the above, since the long side portion can be more freely expanded and thinned due to heating and cooling, it is possible to prevent the mold body from warping due to -aS, and the life of the mold can be extended. ×: Since the tightening force is adjusted to a constant Iz by the leg spring, the attachment can be controlled accurately.

【図面の簡単な説明】[Brief explanation of drawings]

第1図は本願発■の方法で用いる鋳IIの斜視■、第2
図及び第3図け、骨れぐれ締付ポルトの取付状態を示す
説明図、第411mボルト抑通孔が長孔状の物の―劃り 特許出原人 三島光産株式会 代理人を吉教賭 第1!!I − 第2図 第3図 第4図
Figure 1 is a perspective view of Casting II used in the method of the present invention.
Fig. 3 is an explanatory diagram showing the installation state of the bone tightening port, and the 411m bolt holding hole is an elongated hole. Educational bet number 1! ! I - Figure 2 Figure 3 Figure 4

Claims (1)

【特許請求の範囲】[Claims] 1、パックフレームと制置本体とを鋳付ポルトで連結す
るに際し、鋳付ポルトamとパックフレーム間に0リン
グを転装したOリングホルダー及び皿バネを介a′さ曽
、しかも締付ポルトを箇締付ボルト神道孔に遊嵌状にな
らしめたこと壱待徽とする連続鋳造用鋳置メニスカスS
勲疲労堕止方饋。
1. When connecting the pack frame and the control body with the cast port, insert an O-ring holder with an O-ring and a disc spring between the cast port and the pack frame, and also use the tightening port. Foundry meniscus S for continuous casting, which has a loose fit in the Shinto hole of the bolt.
How to stop suffering from fatigue.
JP10367181A 1981-06-30 1981-06-30 Preventing method for thermal fatigue in meniscus part of mold for continuous casting Pending JPS583754A (en)