JPH11278932A - Piezoelectric porcelain - Google Patents

Piezoelectric porcelain

Info

Publication number
JPH11278932A
JPH11278932A JP10086380A JP8638098A JPH11278932A JP H11278932 A JPH11278932 A JP H11278932A JP 10086380 A JP10086380 A JP 10086380A JP 8638098 A JP8638098 A JP 8638098A JP H11278932 A JPH11278932 A JP H11278932A
Authority
JP
Japan
Prior art keywords
piezoelectric
curie temperature
piezoelectric ceramic
substituted
porcelain
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP10086380A
Other languages
Japanese (ja)
Other versions
JP3720572B2 (en
Inventor
Yasuhiro Nakai
泰広 中井
Harumi Hayashi
春美 林
Shuichi Fukuoka
修一 福岡
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kyocera Corp
Original Assignee
Kyocera Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kyocera Corp filed Critical Kyocera Corp
Priority to JP08638098A priority Critical patent/JP3720572B2/en
Publication of JPH11278932A publication Critical patent/JPH11278932A/en
Application granted granted Critical
Publication of JP3720572B2 publication Critical patent/JP3720572B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To obtain non-lead-based piezoelectric porcelain having at least >=100 deg.C high upper limit of temperature used and piezoelectric strain constant (d33 ) in practical level of >=100 pC/N. SOLUTION: This piezoelectric porcelain consists mainly of crystal particles comprising tungsten-bronze type compound oxide represented by the formula; Sr2 NaNb5 O15 and substituting a part of Sr with at least one kind of (Bi1/2 Li1/2 ), (Bi1/2 Na1/2 ) and (Bi1/2 K1/2 ) and at least one kind of element among Mg, Ca and Ba. In the porcelain, it is desirable that a part or all of Na is substituted with K and a part of Nb is substituted with V and/or Ta.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は圧電磁器に関し、精
密工作機械における位置決め、光学装置の光路長制御、
流量制御用バルブ、超音波モータ、あるいは自動車のブ
レーキ装置等に使用するアクチュエータ用の圧電磁器に
関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a piezoelectric ceramic, and relates to positioning in a precision machine tool, control of an optical path length of an optical device,
The present invention relates to a piezoelectric ceramic for an actuator used for a flow control valve, an ultrasonic motor, a brake device of an automobile, or the like.

【0002】[0002]

【従来技術】圧電材料を利用したアクチュエータは、圧
電現象を介して発生する歪み及び力を機械的駆動源とし
て用いるものであり、精密工作機械における位置決め、
光学装置の光路長制御、流量制御用バルブ、超音波モー
タ、あるいは自動車のブレーキ装置等への応用が展開さ
れている。アクチュエータに用いる圧電材料としては、
圧電性に優れるという点からチタン酸ジルコン酸鉛(P
ZT)が最も幅広く利用されてきた。しかしながら、最
近、鉛系廃棄物が酸性雨等に当たると鉛が溶出し、環境
に悪影響を与えることが問題となることから、自重の約
60%の割合で鉛を含有するPZTの代替として利用で
きる鉛を含まない圧電材料が求められている。鉛を含有
しない圧電材料としてBaTiO3 系磁器組成物の利用
が考えられる。例えば、特開平2−159079号公報
及び特開平2−29430号公報では、BaTiO3
圧電磁器組成物を利用することが提案されている。Ba
TiO3 系磁器組成物は、比誘電率(ε33T /ε0 )お
よび電気機械結合係数(k33)が高いという特徴を有
し、300pC/N前後の大きな圧電歪み定数(d33
を示すことから、鉛を含有しないアクチュエータ用の圧
電材料として利用可能である。
2. Description of the Related Art An actuator using a piezoelectric material uses a strain and a force generated through a piezoelectric phenomenon as a mechanical drive source.
Applications to optical path length control of optical devices, flow control valves, ultrasonic motors, automobile brake devices, and the like have been developed. As the piezoelectric material used for the actuator,
Lead zirconate titanate (P
ZT) has been most widely used. However, recently, when lead-based waste is exposed to acid rain or the like, lead is eluted, which has a problem of adversely affecting the environment. Therefore, it can be used as a substitute for PZT containing lead at about 60% of its own weight. There is a need for a piezoelectric material that does not contain lead. As a lead-free piezoelectric material, use of a BaTiO 3 ceramic composition is conceivable. For example, JP-A-2-15979 and JP-A-2-29430 propose to use a BaTiO 3 -based piezoelectric ceramic composition. Ba
The TiO 3 -based porcelain composition is characterized by high relative dielectric constant (ε 33T / ε 0 ) and high electromechanical coupling coefficient (k 33 ), and has a large piezoelectric strain constant (d 33 ) of about 300 pC / N.
Thus, it can be used as a piezoelectric material for a lead-free actuator.

【0003】一方、Ferroelectrics,19
94,Vol160 ,p265 には、Sr2-x Cax NaNb
5 15で表わされるタングステンブロンズ型複合酸化物
の単結晶の比誘電率(ε33T /ε0 )、圧電歪み定数
(d33)、キュリー温度(Tc)について記載されてい
る。この文献によれば、上記単結晶では、比誘電率(ε
33T /ε0 )が1700で、圧電歪み定数(d33)が2
70pC/Nで、キュリー温度(Tc)が270℃とい
う特性を有している。
On the other hand, Ferroelectrics, 19
94, Vol160, the p265 is, Sr 2-x Ca x NaNb
It describes the relative dielectric constant (ε 33T / ε 0 ), piezoelectric strain constant (d 33 ), and Curie temperature (Tc) of a single crystal of a tungsten bronze composite oxide represented by 5 O 15 . According to this document, in the single crystal, the relative dielectric constant (ε
33T / ε 0 ) is 1700 and the piezoelectric distortion constant (d 33 ) is 2
It has a characteristic that the Curie temperature (Tc) is 270 ° C. at 70 pC / N.

【0004】[0004]

【発明が解決しようとする課題】しかしながら、上記特
開平2−159079号公報および特開平2−2943
0号公報におけるBaTiO3 系磁器組成物では、30
0pC/N前後の大きな圧電歪み定数(d33)を有する
磁器組成物を得ることができるが、BaTiO3自身の
キュリー温度(Tc)が約120℃と低く、大きな圧電
歪み定数(d33)を得ようとすると、キュリー温度(T
c)の低下が避けられず、使用温度の上限は100℃よ
りも低下してしまうという問題があった。
However, Japanese Patent Application Laid-Open Nos. 2-159079 and 2-2943 described above.
In the BaTiO 3 -based porcelain composition disclosed in Japanese Patent Publication No.
Although a ceramic composition having a large piezoelectric strain constant (d 33 ) of about 0 pC / N can be obtained, the Curie temperature (Tc) of BaTiO 3 itself is as low as about 120 ° C., and a large piezoelectric strain constant (d 33 ) is obtained. To obtain the Curie temperature (T
There is a problem that the reduction of c) is inevitable, and the upper limit of the operating temperature is lower than 100 ° C.

【0005】一方、本発明者らは、上記文献に記載され
たSr2-x Cax NaNb5 15でで表わされるタング
ステンブロンズ型単結晶と、同様な組成で圧電磁器を作
製したところ、室温での比誘電率(ε33T /ε0 )およ
びキュリー温度(Tc)は単結晶とほぼ同程度の特性を
有するが、圧電歪み定数(d33)が50〜60pC/N
と低くなり、アクチュエータ用の圧電材料としては利用
できるレベルではないことが判った。
On the other hand, the present inventors have prepared a piezoelectric ceramic having the same composition as the tungsten bronze type single crystal represented by Sr 2-x Ca x NaNb 5 O 15 described in the above-mentioned document, and The dielectric constant (ε 33T / ε 0 ) and the Curie temperature (Tc) of the sample are almost the same as those of the single crystal, but the piezoelectric strain constant (d 33 ) is 50 to 60 pC / N.
It was found that this was not at a level usable as a piezoelectric material for an actuator.

【0006】本発明は、使用温度の上限が少なくとも1
50℃以上と高く、100pC/N以上と実用レベルの
圧電歪み定数(d33)を有する非鉛系の圧電磁器を提供
することを目的とする。
According to the present invention, the upper limit of the operating temperature is at least one.
An object of the present invention is to provide a lead-free piezoelectric ceramic having a high piezoelectric strain constant (d 33 ) of as high as 50 ° C. or more and a practical level of 100 pC / N or more.

【0007】[0007]

【課題を解決するための手段】本発明の圧電磁器は、一
般式:Sr2 NaNb5 15で表わされるタングステン
ブロンズ型複合酸化物からなり、Srの一部が(Bi
1/2 Li1/2 )、(Bi1/2 Na1/2 )および(Bi
1/2 1/2 )のうち少なくとも1種と、Mg、Caおよ
びBaのうち少なくとも1種で置換した結晶粒子を主体
とするものである。
The piezoelectric ceramic according to the present invention is made of a tungsten bronze type composite oxide represented by the general formula: Sr 2 NaNb 5 O 15 , and a part of Sr is (Bi)
1/2 Li 1/2 ), (Bi 1/2 Na 1/2 ) and (Bi
1/2 K 1/2 ) and crystal grains substituted by at least one of Mg, Ca and Ba.

【0008】ここで、Naの一部または全部がKで置換
されるとともに、Nbの一部がVおよび/またはTaで
置換されていることが望ましい。
Here, it is desirable that part or all of Na is substituted with K and part of Nb is substituted with V and / or Ta.

【0009】本発明の圧電磁器は、原子比による組成式
を (Sr2-(a+b) a b x (Na1-c c y (Nb
5-d d )O15 と表わした時、前記a、b、c、d、xおよびyが、
0.10≦a≦0.65、0<b≦0.40、0≦c≦
1.0、CがVの時0≦d≦0.10、CがTaの時0
≦d≦0.50、0.96≦x≦1.04、0.80≦
y≦1.20を満足することが望ましい。ここで、A
は、Mg、CaおよびBaのうち少なくとも1種であ
り、Bは、(Bi1/2 Li1/2 )、(Bi1/2
1/2 )および(Bi1/ 2 1/2 )のうち少なくとも1
種を示す。
[0009] The piezoelectric ceramic of the present invention, the composition formula by atomic ratio (Sr 2- (a + b) A a B b) x (Na 1-c K c) y (Nb
5-d C d ) O 15 , wherein a, b, c, d, x and y are
0.10 ≦ a ≦ 0.65, 0 <b ≦ 0.40, 0 ≦ c ≦
1.0, 0 ≦ d ≦ 0.10 when C is V, 0 when C is Ta
≦ d ≦ 0.50, 0.96 ≦ x ≦ 1.04, 0.80 ≦
It is desirable to satisfy y ≦ 1.20. Where A
Is at least one of Mg, Ca and Ba, and B is (Bi 1/2 Li 1/2 ), (Bi 1/2 N
a 1/2) and at least one of (Bi 1/2 K 1/2)
Indicates the species.

【0010】[0010]

【作用】本発明の圧電磁器は、一般式:Sr2 NaNb
5 15で表わされるタングステンブロンズ型複合酸化物
からなり、Srの一部が(Bi1/2 Li1/2 )、(Bi
1/2 Na1/2 )および(Bi1/2 1/2 )のうち少なく
とも1種と、Mg、CaおよびBaのうち少なくとも一
種で置換した結晶粒子を主体とするため、キュリー温度
(Tc)が150℃以上と高く、圧電歪み定数(d33
が100pC/N以上と実用的レベルまで向上できる。
The piezoelectric ceramic of the present invention has a general formula: Sr 2 NaNb
It is composed of a tungsten bronze-type composite oxide represented by 5 O 15 , and a part of Sr is (Bi 1/2 Li 1/2 ), (Bi
1/2 Na 1/2 ) and (Bi 1/2 K 1/2 ) and at least one of Mg, Ca and Ba replaced by crystal grains, so that the Curie temperature (Tc ) Is as high as 150 ° C. or higher, and the piezoelectric strain constant (d 33 )
Can be improved to a practical level of 100 pC / N or more.

【0011】また、本発明の圧電磁器は、環境に悪影響
を与える鉛を含有せず、大気中で焼成できるので製造が
容易である。
Further, the piezoelectric ceramic of the present invention does not contain lead, which has an adverse effect on the environment, and can be fired in the air, so that it is easy to manufacture.

【0012】さらに、Naの一部または全部をKで置換
するとともに、Nbの一部をVおよび/またはTaで置
換することにより、比誘電率(ε33T /ε0 )および電
気機械結合係数(k33)を向上して圧電歪み定数
(d33)をさらに高くできる。
Further, by substituting a part or all of Na with K and substituting a part of Nb with V and / or Ta, the relative dielectric constant (ε 33T / ε 0 ) and the electromechanical coupling coefficient ( k 33 ) can be improved to further increase the piezoelectric distortion constant (d 33 ).

【0013】[0013]

【発明の実施の形態】本発明の圧電磁器は、一般式:S
2 NaNb5 15で表わされるタングステンブロンズ
型複合酸化物であって、Srの一部が(Bi1/2 Li
1/2 )、(Bi1/2 Na1/2 )および(Bi
1/2 1/2 )のうち少なくとも1種と、Mg、Caおよ
びBaのうち少なくとも一種で置換した結晶粒子を主体
とするものである。
DESCRIPTION OF THE PREFERRED EMBODIMENTS A piezoelectric ceramic of the present invention has a general formula: S
A tungsten bronze composite oxide represented by r 2 NaNb 5 O 15 , wherein a part of Sr is (Bi 1/2 Li
1/2 ), (Bi 1/2 Na 1/2 ) and (Bi
1/2 K 1/2 ) and crystal grains substituted with at least one of Mg, Ca and Ba.

【0014】このように従来知られているSr2 NaN
5 15の一部を(Bi1/2 Li1/2)、(Bi1/2
1/2 )および(Bi1/2 1/2 )と、Mg、Caおよ
びBaのうち少なくとも一種で置換することにより、比
誘電率(ε33T /ε0 )および電気機械結合係数
(k33)を高くできる。また、Naの一部または全部を
Kで置換するとともに、Nbの一部をVおよび/または
Taで置換することが望ましい。このように置換するこ
とによって、比誘電率(ε33T /ε0 )および電気機械
結合係数(k33)を向上して、圧電歪み定数(d33)を
さらに高くできる。
Thus, the conventionally known Sr 2 NaN
Part of b 5 O 15 is (Bi 1/2 Li 1/2 ), (Bi 1/2 N
a 1/2 ) and (Bi 1/2 K 1/2 ) and at least one of Mg, Ca and Ba, thereby obtaining a relative dielectric constant (ε 33T / ε 0 ) and an electromechanical coupling coefficient (k). 33 ) can be higher. In addition, it is desirable to partially or entirely replace Na with K and partially replace Nb with V and / or Ta. By such substitution, the relative dielectric constant (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ) are improved, and the piezoelectric strain constant (d 33 ) can be further increased.

【0015】本発明の圧電磁器では、特に、原子比によ
る組成式を(Sr2-(a+b) a bx (Na
1-c c y (Nb5-d d )O15と表した時、前記
a、b、c、d、xおよびyが、0.10≦a≦0.6
5、0<b≦0.40、0≦c≦1.00.96≦x≦
1.04、0.80≦y≦1.20を満足し、CがVの
場合には0≦d≦0.10、CがTaの場合には0≦d
≦0.50を満足することが望ましい。ここで、AはM
g、CaおよびBaのうち少なくとも1種であり、Bは
(Bi1/2 Li1/2 )、(Bi1/2 Na1/2 )および
(Bi1/2 1/2 )のうち少なくとも1種である。
In the piezoelectric ceramic of the present invention, in particular, the composition formula based on the atomic ratio is represented by (Sr 2− (a + b) A a B b ) x (Na
1-cK c ) y (Nb 5-d C d ) O 15 , a, b, c, d, x and y are 0.10 ≦ a ≦ 0.6
5, 0 <b ≦ 0.40, 0 ≦ c ≦ 1.00.96 ≦ x ≦
1.04, 0.80 ≦ y ≦ 1.20, 0 ≦ d ≦ 0.10 when C is V, and 0 ≦ d when C is Ta
It is desirable to satisfy ≦ 0.50. Where A is M
g, at least one of Ca and Ba, and B is at least one of (Bi1 / 2Li1 / 2 ), (Bi1 / 2Na1 / 2 ) and (Bi1 / 2K1 / 2 ). One kind.

【0016】ここで、aを0.10≦a≦0.65の範
囲とした理由は、aが0.10未満である場合には比誘
電率(ε33T /ε0 )および電気機械結合係数(k33
が低下し、aが0.65よりも大きい場合には比誘電率
(ε33T /ε0 )が低下するからである。比誘電率(ε
33T /ε0 )および電気機械結合係数(k33)に優れる
という点からaは0.20≦a≦0.50であることが
望ましい。
Here, the reason why a is set in the range of 0.10 ≦ a ≦ 0.65 is that when a is less than 0.10, the relative dielectric constant (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33)
This is because when a is larger than 0.65, the relative dielectric constant (ε 33T / ε 0 ) decreases. Relative permittivity (ε
A is preferably 0.20 ≦ a ≦ 0.50 from the viewpoint of excellent 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ).

【0017】上記主成分において、bを0<b≦0.4
0の範囲とした理由は、この範囲においてキュリー温度
(Tc)が高く、高い比誘電率(ε33T /ε0 )および
電気機械結合係数(k33)を有する磁器を得ることがで
きるからである。bが大きくなるに従って、キュリー温
度(Tc)は低下するが、比誘電率(ε33T /ε0 )お
よび電気機械結合係数(k33)が顕著に向上するという
効果がある。bは、特に、キュリー温度(Tc)が高
く、比誘電率(ε33T /ε0 )および電気機械結合係数
(k33)に優れるという点から、bは0<b≦0.30
であることが望ましい。
In the above main component, b is 0 <b ≦ 0.4.
The reason for setting the range to 0 is that in this range, it is possible to obtain a porcelain having a high Curie temperature (Tc) and a high relative dielectric constant (ε 33T / ε 0 ) and an electromechanical coupling coefficient (k 33 ). . As b increases, the Curie temperature (Tc) decreases, but the relative permittivity (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ) are significantly improved. In particular, b is 0 <b ≦ 0.30 in that it has a high Curie temperature (Tc) and is excellent in relative permittivity (ε 33T / ε 0 ) and electromechanical coupling coefficient (k 33 ).
It is desirable that

【0018】また、上記一般式において、Naの一部を
Kで置換するとキュリー温度(Tc)は低下するが、比
誘電率(ε33T /ε0 )および電気機械結合係数
(k33)が向上するという効果がある。キュリー温度
(Tc)が高く、比誘電率(ε33T /ε0 )および電気
機械結合係数(k33)に優れるという点から、NaとK
の割合を表わすcは、0.5≦c≦0.80の範囲であ
ることが望ましい。
In the above general formula, when a part of Na is replaced with K, the Curie temperature (Tc) decreases, but the relative dielectric constant (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ) increase. There is an effect of doing. Na and K have high Curie temperature (Tc) and are excellent in relative dielectric constant (ε 33T / ε 0 ) and electromechanical coupling coefficient (k 33 ).
Is preferably in the range of 0.5 ≦ c ≦ 0.80.

【0019】さらに、上記一般式において、Nbの一部
を特定の金属元素C(VおよびTaのうち少なくとも1
種)で置換すると、さらに圧電歪み定数(d33)を向上
することができる。Nbの一部をVで置換する場合に
は、キュリー温度(Tc)および電気機械結合係数(k
33)が向上するという効果がある。しかしながら、Vで
置換し過ぎると焼結性の悪化を招くので、dは0≦d≦
0.10の範囲であることが望ましい。一方、Nbの一
部をTaで置換する場合には、キュリー温度(Tc)は
低下するが、比誘電率(ε33T /ε0 )および電気機械
結合係数(k33)が向上するという効果が認められる。
キュリー温度(Tc)が高く、比誘電率(ε33T
ε0 )および電気機械結合係数(k33)に優れるという
点から、Taで置換した場合には、dは0.50以下で
あることが望ましい。特に、キュリー温度(Tc)が高
く、大きな圧電歪み定数(d33)を示すという点から、
Nbの一部をVで置換する場合のdの範囲は0.02≦
d≦0.04であることが望ましく、Taで置換する場
合のdの範囲は0.20≦d≦0.40であることが望
ましい。
Further, in the above general formula, a part of Nb is replaced with a specific metal element C (at least one of V and Ta).
Substituting with (seed) can further improve the piezoelectric distortion constant (d 33 ). When a part of Nb is replaced by V, the Curie temperature (Tc) and the electromechanical coupling coefficient (k
33 ) has the effect of improving. However, excessive substitution with V causes deterioration of the sinterability, so that d is 0 ≦ d ≦
It is desirable to be in the range of 0.10. On the other hand, when a part of Nb is replaced with Ta, the Curie temperature (Tc) decreases, but the relative permittivity (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ) improve. Is recognized.
Curie temperature (Tc) is high and relative dielectric constant (ε 33T /
From the viewpoint of excellent ε 0 ) and electromechanical coupling coefficient (k 33 ), d is desirably 0.50 or less when substituted with Ta. In particular, the Curie temperature (Tc) is higher, in terms of showing the large piezoelectric strain constant (d 33),
When a part of Nb is replaced by V, the range of d is 0.02 ≦
It is preferable that d ≦ 0.04, and the range of d when Ta is substituted is 0.20 ≦ d ≦ 0.40.

【0020】さらに、上記主成分におけるxを0.96
≦x≦1.04とした理由は、xが0.96未満である
場合には磁器中に異相が生じ易く、圧電歪み定数
(d33)が低下し、1.04よりも大きい場合には磁器
の焼結性が悪化するために圧電歪み定数(d33)が小さ
くなるからである。一方、y を0.80≦y≦1.20
の範囲とした理由は、yが0.80未満である場合に
は、比誘電率(ε33T /ε0 )および電気機械結合係数
(k33)が共に低下し、yが1.20よりも大きい場合
は、磁器の焼結性が悪化し、主として電気機械結合係数
(k33)が低下するからである。磁器の焼結が良く、大
きい圧電歪み定数(d33)を示すという点から、xは
0.98≦x≦1.02、y は0.90≦y≦1.10
の範囲であることが特に望ましい。
Further, x in the above main component is 0.96.
The reason for ≦ x ≦ 1.04 is that when x is less than 0.96, a different phase is likely to occur in the porcelain, the piezoelectric strain constant (d 33 ) decreases, and when x is greater than 1.04, This is because the sinterability of the porcelain deteriorates, and the piezoelectric distortion constant (d 33 ) decreases. On the other hand, y is set to 0.80 ≦ y ≦ 1.20
The reason is that when y is less than 0.80, both the relative dielectric constant (ε 33T / ε 0 ) and the electromechanical coupling coefficient (k 33 ) decrease, and y is larger than 1.20. If it is large, the sinterability of the porcelain deteriorates, and mainly the electromechanical coupling coefficient (k 33 ) decreases. X is 0.98 ≦ x ≦ 1.02, and y is 0.90 ≦ y ≦ 1.10, since the porcelain has good sintering and exhibits a large piezoelectric strain constant (d 33 ).
Is particularly desirable.

【0021】なお、本発明の圧電磁器は、一般式:(S
2-(a+b) a b x (Na1-cc y (Nb5-d
d )O15で表されるタングステンブロンズ型結晶相を
主結晶相とするものであり、金属元素の大部分が上記主
結晶相に固溶した結晶相となる。本発明の圧電磁器で
は、Rb、Ce、Fe、Al、Si等の不可避不純物が
混入する場合がある。また、プレス成形の金型等から、
Ni、Cr、Mo、Ni等の金属元素が混入する場合も
ある。さらに、温度特性や耐熱性を向上するために、C
u、Mn、Cr、Co等を添加しても良い。
The piezoelectric ceramic of the present invention has a general formula: (S
r 2- (a + b) A a B b) x (Na 1-c K c) y (Nb 5-d
C d ) A tungsten bronze-type crystal phase represented by O 15 is used as a main crystal phase, and most of the metal elements are in a solid solution with the main crystal phase. In the piezoelectric ceramic of the present invention, inevitable impurities such as Rb, Ce, Fe, Al, and Si may be mixed. Also, from press molding dies, etc.,
In some cases, metal elements such as Ni, Cr, Mo, and Ni are mixed. Furthermore, in order to improve temperature characteristics and heat resistance, C
u, Mn, Cr, Co, etc. may be added.

【0022】本発明の圧電磁器は、例えば、次のように
して製造することができる。先ず、SrCO3 、MgC
3 、CaCO3 、BaCO3 、Bi2 3 、Li2
3、Na2 CO3 、K2 CO3 、Nb2 5 、V2
5 、Ta2 5 の各粉末を所定の割合で混合し、900
〜1100℃で2〜5時間仮焼した後、粉砕することに
より所望の組成の圧電材料の粉末を得る。この粉末に有
機バインダーを混合し、金型プレス、静水圧プレス等に
より所望の形状に成形した後、1200〜1280℃で
2〜5時間焼成することにより磁器を得る。これを必要
に応じて所望の厚さに加工して使用する。
The piezoelectric ceramic of the present invention can be manufactured, for example, as follows. First, SrCO 3 , MgC
O 3 , CaCO 3 , BaCO 3 , Bi 2 O 3 , Li 2 C
O 3 , Na 2 CO 3 , K 2 CO 3 , Nb 2 O 5 , V 2 O
5 , each powder of Ta 2 O 5 is mixed at a predetermined ratio and 900
After calcining at 11100 ° C. for 2 to 5 hours, the resultant is crushed to obtain a piezoelectric material powder having a desired composition. An organic binder is mixed with the powder, molded into a desired shape by a die press, an isostatic press or the like, and then fired at 1200 to 1280 ° C. for 2 to 5 hours to obtain a porcelain. This is processed to a desired thickness as needed and used.

【0023】なお、SrCO3 、MgCO3 、CaCO
3 、BaCO3 、Bi2 3 、Li2 CO3 、Na2
3 、K2 CO3 、Nb2 5 、V2 5 、Ta2 5
粉末は、それぞれの金属元素を含有する酸化物、炭酸
塩、酢酸塩等の化合物、もしくは有機金属等の化合物の
いずれであっても、焼成により酸化物となるものであれ
ば問題ない。
Note that SrCO 3 , MgCO 3 , CaCO
3 , BaCO 3 , Bi 2 O 3 , Li 2 CO 3 , Na 2 C
O 3 , K 2 CO 3 , Nb 2 O 5 , V 2 O 5 , Ta 2 O 5
The powder may be any of oxides, carbonates, acetates, and other compounds containing the respective metal elements, or compounds of organic metals and the like, as long as they become oxides by firing.

【0024】[0024]

【実施例】出発原料として、SrCO3 、MgCO3
CaCO3 、BaCO3 、Bi23 、Na2 CO3
2 CO3 、Nb2 5 、V2 5 、Ta2 5 、粉末
を用いて、焼結体組成が、モル比による組成式:(Sr
2-(a+b) a b x (Na1-c c y (Nb5-d
d )O15におけるa、b、c、d、x及びyが表1に示
す値となるように秤量した。この混合物をZrO2 ボー
ルを用いたボールミルで12時間湿式混合した。次い
で、この混合物を乾燥した後、大気中で900〜110
0℃で3時間仮焼し、該仮焼物を再び上記ボールミルで
粉砕した。その後、この粉砕物にバインダー(PVA)
を混合して造粒した。得られた粉末を1.5t/cm2
の圧力で直径5mm、厚さ8mmの寸法からなる円柱に
プレス成形した。
EXAMPLES As starting materials, SrCO 3 , MgCO 3 ,
CaCO 3 , BaCO 3 , Bi 2 O 3 , Na 2 CO 3 ,
Using K 2 CO 3 , Nb 2 O 5 , V 2 O 5 , Ta 2 O 5 , and powder, the composition of the sintered body is determined by a molar ratio of a composition formula: (Sr
2- (a + b) A a B b) x (Na 1-c K c) y (Nb 5-d C
d ) It was weighed so that a, b, c, d, x and y at O 15 became the values shown in Table 1. This mixture was wet-mixed in a ball mill using ZrO 2 balls for 12 hours. Next, after drying this mixture, 900-110
The calcined product was calcined at 0 ° C. for 3 hours, and the calcined product was pulverized again by the ball mill. Then, a binder (PVA) is added to the pulverized material.
Was mixed and granulated. 1.5 t / cm 2 of the obtained powder
At a pressure of 5 mm to form a cylinder having a diameter of 5 mm and a thickness of 8 mm.

【0025】これらの成形体をMgOからなる板に並
べ、大気中において1200℃〜1280℃の範囲で2
〜5時間焼成した。得られた磁器について、X 線回折の
測定による測定を行ったところ、本発明の試料では、S
2 NaNb5 15またはSr2 KNb5 15で表され
るタングステンブロンズ型複合酸化物からなり、(Bi
1/2 Li1/2 )、(Bi1/2 Na1/2 )および(Bi
1/2 1/2 )の少なくとも一種と、Mg、CaおよびB
aの少なくとも一種、もしくはさらにVまたはTaが固
溶した結晶相を主体とすることを確認した。
These compacts are arranged on a plate made of MgO, and are heated at 1200 ° C. to 1280 ° C. in the air.
Fired for ~ 5 hours. The obtained porcelain was measured by X-ray diffraction measurement.
a tungsten bronze-type composite oxide represented by r 2 NaNb 5 O 15 or Sr 2 KNb 5 O 15;
1/2 Li 1/2 ), (Bi 1/2 Na 1/2 ) and (Bi
1/2 K 1/2 ), Mg, Ca and B
It was confirmed that at least one of a, or a crystal phase in which V or Ta was dissolved was mainly used.

【0026】得られた圧電磁器に銀電極を焼き付け、1
20〜150℃のシリコンオイル中で5〜8kV/mm
の直流電界を印加して分極処理した。そして比誘電率
(ε33 T /ε0 )および縦方向の共振・反共振周波数を
室温下においてインピーダンスアナライザーを用いて測
定し、電気機械結合係数(k33)及び弾性コンプライア
ンス(S33E )を算出し、磁器の圧電歪み定数(d33
を求めた。
A silver electrode is baked on the obtained piezoelectric ceramic,
5 to 8 kV / mm in silicon oil at 20 to 150 ° C
Was applied to perform polarization processing. The relative permittivity (ε 33 T / ε 0 ) and the longitudinal resonance / anti-resonance frequency are measured at room temperature using an impedance analyzer to calculate the electromechanical coupling coefficient (k 33 ) and the elastic compliance (S 33E ). and, porcelain piezoelectric strain constant (d 33)
I asked.

【0027】また、上記圧電磁器の比誘電率(ε33T
ε0 )を温度の関数としてプロットすることにより強誘
電相と常誘電相の相転移点の温度(キュリー温度(T
c))を求めた。これらの結果を表2に記載した。
Further, the relative permittivity (ε 33T /
By plotting ε 0 ) as a function of temperature, the temperature at the phase transition point between the ferroelectric phase and the paraelectric phase (Curie temperature (T
c)) was determined. These results are shown in Table 2.

【0028】[0028]

【表1】 [Table 1]

【0029】[0029]

【表2】 [Table 2]

【0030】これらの表1、2より、本発明の試料では
何れも150℃よりも高いキュリー温度(Tc)を有し
ているのがわかる。しかも、圧電歪み定数(d33)が1
00pC/N以上、特には150pC/N以上と優れて
おり、圧電磁器として実用的レベルにあることが判る。
From Tables 1 and 2, it can be seen that the samples of the present invention all have a Curie temperature (Tc) higher than 150 ° C. Moreover, the piezoelectric strain constant (d 33 ) is 1
It is excellent at 00 pC / N or more, particularly 150 pC / N or more, and it can be seen that it is at a practical level as a piezoelectric ceramic.

【0031】一方、Sr2 NaNb5 15の一部をCa
で置換した従来の組成では、圧電歪み定数(d33)が5
9pC/Nと低いことが判る(試料No.1)。
On the other hand, a part of Sr 2 NaNb 5 O 15 is converted to Ca
In the conventional composition substituted by the above, the piezoelectric strain constant (d 33 ) is 5
It turns out that it is as low as 9 pC / N (sample No. 1).

【0032】また、SrのMg、Ca、Baによる置換
量aが0.10から0.65の間で圧電歪み定数
(d33)のピークを有するのが判る(試料No.19〜
23)。Srの(Bi1/2 Li1/2 )、(Bi1/2 Na
1/2 )および(Bi1/2 1/2 )による置換量bが増加
すると、キュリー温度(Tc)が低下し、圧電歪み定数
(d33)が向上するのが判る(試料No.2〜5)。
Further, it can be seen that the substitution amount a of Sr with Mg, Ca, and Ba has a peak of the piezoelectric strain constant (d 33 ) between 0.10 and 0.65 (sample Nos. 19 to 19).
23). (Bi 1/2 Li 1/2 ), (Bi 1/2 Na)
It can be seen that the Curie temperature (Tc) decreases and the piezoelectric strain constant (d 33 ) increases as the amount of substitution b by ( 1/2 ) and (Bi 1/2 K 1/2 ) increases (Sample No. 2). ~ 5).

【0033】さらに、Naの一部をKで置換すると、キ
ュリー温度(Tc)が低下し、圧電歪み定数(d33)が
さらに向上するのが判る(試料No.15〜18)。
Further, it can be seen that when a part of Na is replaced with K, the Curie temperature (Tc) is lowered and the piezoelectric strain constant (d 33 ) is further improved (Sample Nos. 15 to 18).

【0034】また、NbのVによる置換量dが0.01
〜0.10の間で圧電歪み定数(d33)のピークを有
し、キュリー温度(Tc)が次第に高くなることが判る
(試料No.6〜10)。一方、NbのTaによる置換
量dが大きくなるに従って、圧電歪み定数(d33)が次
第に高くなるが、キュリー温度(Tc)が低下すること
が判る(試料No.11〜14)。
The replacement amount d of Nb by V is 0.01
It has a peak of the piezoelectric strain constant (d 33 ) between の 間 0.10 and the Curie temperature (Tc) gradually increases (samples Nos. 6 to 10). On the other hand, as the substitution amount d of Nb with Ta increases, the piezoelectric strain constant (d 33 ) gradually increases, but the Curie temperature (Tc) decreases (samples Nos. 11 to 14).

【0035】一方、xが0.96〜1.04の間で圧電
歪み定数(d33)のピークが存在し、かつ、xの増加に
伴ってキュリー温度(Tc)が次第に高くなるのが判る
(試料No.24〜28)。yが0.80〜1.20の
間で圧電歪み定数(d33)のピークが存在し、yの増加
に伴ってキュリー温度(Tc)が次第に高くなるのが判
る(試料No.29〜32)。
On the other hand, it can be seen that a peak of the piezoelectric strain constant (d 33 ) exists when x is between 0.96 and 1.04, and that the Curie temperature (Tc) gradually increases as x increases. (Sample Nos. 24 to 28). y is a peak exists in the piezoelectric strain constant (d 33) between 0.80 to 1.20, the Curie temperature (Tc) is gradually to be seen higher with an increase of y (sample No.29~32 ).

【0036】また、試料No.33〜35では、200
℃と高いキュリー温度(Tc)を有するにも関わらず、
120pC/N以上と圧電歪み定数(d33)に優れるこ
とが判る。尚、表1において、BiLi、BiNa、B
iKとは、(Bi1/2 Li1/ 2 )、(Bi1/2
1/2 )、(Bi1/2 1/2 )を示す。
Sample No. For 33-35, 200
Despite having a high Curie temperature (Tc) of ℃
It can be seen that the piezoelectric strain constant (d 33 ) is excellent at 120 pC / N or more. In Table 1, BiLi, BiNa, B
The iK, (Bi 1/2 Li 1/ 2), (Bi 1/2 N
a 1/2 ) and (Bi 1/2 K 1/2 ).

【0037】[0037]

【発明の効果】以上のように、本発明による圧電磁器に
よれば、キュリー温度(Tc)が150℃よりも高く、
100pC/N以上の圧電歪み定数(d33)を有し、積
層型アクチュエータ用の圧電材料として実用化できるレ
ベルの非鉛系圧電磁器が提供できる。鉛を含有していな
いので、酸性雨による鉛の溶出により環境に悪影響を与
えることがない。
As described above, according to the piezoelectric ceramic of the present invention, the Curie temperature (Tc) is higher than 150 ° C.
A lead-free piezoelectric ceramic having a piezoelectric strain constant (d 33 ) of 100 pC / N or more and practically usable as a piezoelectric material for a laminated actuator can be provided. Since it does not contain lead, it does not adversely affect the environment due to elution of lead by acid rain.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】一般式:Sr2 NaNb5 15で表わされ
るタングステンブロンズ型複合酸化物からなり、Srの
一部が(Bi1/2 Li1/2 )、(Bi1/2 Na1/2 )お
よび(Bi1/2 1/2 )のうち少なくとも1種と、M
g、CaおよびBaのうち少なくとも1種で置換した結
晶粒子を主体とすることを特徴とする圧電磁器。
1. A tungsten bronze composite oxide represented by the general formula: Sr 2 NaNb 5 O 15 , wherein part of Sr is (Bi 1/2 Li 1/2 ) or (Bi 1/2 Na 1 / 2 ) and at least one of (Bi 1/2 K 1/2 ) and M
A piezoelectric ceramic mainly comprising crystal grains substituted with at least one of g, Ca and Ba.
【請求項2】Naの一部または全部がKで置換されると
ともに、Nbの一部がVおよび/またはTaで置換され
ていることを特徴とする請求項1記載の圧電磁器。
2. The piezoelectric ceramic according to claim 1, wherein a part or all of Na is substituted with K and a part of Nb is substituted with V and / or Ta.
【請求項3】原子比による組成式を (Sr2-(a+b) a b x (Na1-c c y (Nb
5-d d )O15 と表わした時、前記a、b、c、d、xおよびyが 0.10≦a≦0.65 0<b≦0.40 0≦c≦1.0 0≦d≦0.10 0.96≦x≦1.04 0.80≦y≦1.20 A・・・ Mg、CaおよびBaのうち少なくとも1
種。 B・・・(Bi1/2 Li1/2 )、(Bi1/2 Na1/2
および(Bi1/21/2 )のうち少なくとも1種 を満足することを特徴とする請求項1または2記載の圧
電磁器。
3. A formula according to the atomic ratio (Sr 2- (a + b) A a B b) x (Na 1-c K c) y (Nb
5-dV d ) O 15 , where a, b, c, d, x and y are 0.10 ≦ a ≦ 0.65 0 <b ≦ 0.40 0 ≦ c ≦ 1.00 ≦ d ≦ 0.10 0.96 ≦ x ≦ 1.04 0.80 ≦ y ≦ 1.20 A ... At least one of Mg, Ca and Ba
seed. B: (Bi 1/2 Li 1/2 ), (Bi 1/2 Na 1/2 )
The piezoelectric ceramic according to claim 1 or 2, wherein at least one of (Bi1 / 2K1 / 2 ) is satisfied.
【請求項4】原子比による組成式を (Sr2-(a+b) a b x (Na1-c c y (Nb
5-d Tad )O15 と表わした時、前記a、b、c、d、xおよびyが 0.10≦a≦0.65 0<b≦0.40 0≦c≦1.0 0≦d≦0.50 0.96≦x≦1.04 0.80≦y≦1.20 A・・・ Mg、CaおよびBaのうち少なくとも1
種。 B・・・(Bi1/2 Li1/2 )、(Bi1/2 Na1/2
および(Bi1/21/2 )のうち少なくとも1種 を満足することを特徴とする請求項1または2記載の圧
電磁器。
Wherein the composition formula by atomic ratio (Sr 2- (a + b) A a B b) x (Na 1-c K c) y (Nb
5-d Ta d ) O 15 where a, b, c, d, x and y are 0.10 ≦ a ≦ 0.65 0 <b ≦ 0.40 0 ≦ c ≦ 1.00 ≦ d ≦ 0.50 0.96 ≦ x ≦ 1.04 0.80 ≦ y ≦ 1.20 A ... At least one of Mg, Ca and Ba
seed. B: (Bi 1/2 Li 1/2 ), (Bi 1/2 Na 1/2 )
The piezoelectric ceramic according to claim 1 or 2, wherein at least one of (Bi1 / 2K1 / 2 ) is satisfied.
JP08638098A 1998-03-31 1998-03-31 Piezoelectric ceramic Expired - Fee Related JP3720572B2 (en)