JPH0643600B2 - 分散安定性の優れた液状クレンザ−組成物 - Google Patents

分散安定性の優れた液状クレンザ−組成物

Info

Publication number
JPH0643600B2
JPH0643600B2 JP1316686A JP1316686A JPH0643600B2 JP H0643600 B2 JPH0643600 B2 JP H0643600B2 JP 1316686 A JP1316686 A JP 1316686A JP 1316686 A JP1316686 A JP 1316686A JP H0643600 B2 JPH0643600 B2 JP H0643600B2
Authority
JP
Japan
Prior art keywords
liquid cleanser
dispersion stability
cleanser composition
excellent dispersion
cmc
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP1316686A
Other languages
English (en)
Other versions
JPS62172099A (ja
Inventor
武夫 大宮
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Daicel Corp
Original Assignee
Daicel Chemical Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Daicel Chemical Industries Ltd filed Critical Daicel Chemical Industries Ltd
Priority to JP1316686A priority Critical patent/JPH0643600B2/ja
Publication of JPS62172099A publication Critical patent/JPS62172099A/ja
Publication of JPH0643600B2 publication Critical patent/JPH0643600B2/ja
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【発明の詳細な説明】 (産業上の利用分野) 本発明は分散安定性の優れた液状クレンザー組成物に関
するものである。
(従来の技術及び問題点) 従来、この種の製品は、研摩材をスラリー化するために
界面活性剤を用いているから、温度に対する安定性が不
十分で、低温領域においてしばしば分離現象が発生する
のを避けられなかった。
(本発明の目的) 本発明は、前述の問題点を解決し得る分散安定性の優れ
た液状クレンザー組成物を提供せんとするものである。
(発明の構成及び効果) 以下、本発明の液状クレンザー組成物を説明する。本発
明の組成物は研摩材を主成分としてこれを置換度(以下
DSと略称する)1.3以上のカルボキシメチルセルロ
ースエーテルアルカリ金属塩(以下CMCと略称する)
80〜20重量%と微小フイブリル化セルロース20〜
80重量%(以下MFCと略称する)との複合体並びに
無定形シリカで分散せしめ、更に、この溶液中にアルコ
ール類を混入した事を特徴とするものである。
本発明液状クレンザー組成物は、上記の如くCMCとM
FCの複合体で増粘させて、研摩材粒子を分散させると
共に、無定形シリカの三次元立体構造性を利用して、研
摩材粒子を立体構造内に封入する事により研摩材粒子の
分散状態を維持するものであり、更に、また上記アルコ
ール類により、凍結解凍後における研摩材粒子の分離を
防止するものであるから、研摩材粒子の分散を均一に行
なえる他、低温領域における分離現象を確実に防止する
事が出来る効果がある。
そしてまた、アルコール類はエチレングリコール、ポリ
エチレングリコール、ブチレングリコール、プロピレン
グリコールなどが挙げられこの内プロピレングリコール
は無定形シリカの性能を向上せしめる特長があるから、
これによって研摩材粒子の分散を更に、良好に維持出来
る点から好ましく使用される。
なお、本発明に使用するCMCとMFCの複合体の一成
分であるMFCは精製したセルロース原料を水に懸濁さ
せ、高温、高圧下に特殊な機械的処理を加えて製造され
るものであり、セルロース繊維を微小繊維化したセルロ
ース分約2〜3%、水97〜98%からなるペースト状
の水懸濁液である。
また、CMCとMFC複合体は、上記のMFCにCMC
を添加混合して溶解させた物を乾燥、粉砕して粉末状と
したものである。
このCMCとMFCの複合体は、CMC単独のものに比
して研摩材等の分散安定性及び増粘性の点において優れ
ている。
このCMCとMFCの複合体の重量組成比は8:2〜
2:8、好しくは7:3〜3:7で優れた分散安定性を
発揮する。
また、研摩材としては人造と天然との2種があるが、人
造品が多く使用される。天然品としてザクロ石、金剛
石、ケイ砂などが挙げられ、人造品としては、酸化アル
ミニウム、炭化ケイ素、炭化ホウ素、酸化セリウム、酸
化クロム、酸化ジルコニウム、酸化鉄、人造ダイヤモン
ドなどが挙げられ、通常これらを単独または適宜混合し
て使用する。
なお、この複合体に使用するCMCはDS1.3以上、
好しくは1.8以上のものを用いることによって、経日
安定性の良い液体クレンザーが得られる。これはCMC
のDSが高くなるに従って、耐腐敗性が向上するためで
ある。
本液状クレンザー組成物には、公知の界面活性剤、例え
ばDBSやその他の物質、例えば香料、色素等が所望に
より添加される。
以下に実施例を示す。尚%比は重量基準を示す。
(実施例) 研摩材(ケイ砂50%と酸化鉄50%の混合 物) 40〜60% DS1.4のCMCとMFC6:4の複合体 0.2〜0.7% プロピレングリコール 2〜6% ドデシルベンゼンスルホン酸ソーダ 適 量 無定形シリカ 残 部 計 100.0% 本実施例により得られた組成物を30回反復して凍結解
凍したところ、異常を生じない事が判明した。
本発明の液状クレンザー組成物は上述の如きものである
から、この種の製品として効果のあるものである。

Claims (1)

    【特許請求の範囲】
  1. 【請求項1】主成分の研摩材に置換度1.3以上のカル
    ボキシメチルセルロースエーテルアルカリ金属塩80〜2
    0重量%と微小フイブリル化セルロース20〜80重量%
    との複合体並びに無定形シリカ及びアルコール類を添加
    して成ることを特徴とする分散安定性の優れた液状クレ
    ンザー組成物
JP1316686A 1986-01-24 1986-01-24 分散安定性の優れた液状クレンザ−組成物 Expired - Lifetime JPH0643600B2 (ja)