JP7336071B2 - Sheet glass manufacturing method and its manufacturing apparatus - Google Patents

Sheet glass manufacturing method and its manufacturing apparatus Download PDF

Info

Publication number
JP7336071B2
JP7336071B2 JP2019185419A JP2019185419A JP7336071B2 JP 7336071 B2 JP7336071 B2 JP 7336071B2 JP 2019185419 A JP2019185419 A JP 2019185419A JP 2019185419 A JP2019185419 A JP 2019185419A JP 7336071 B2 JP7336071 B2 JP 7336071B2
Authority
JP
Japan
Prior art keywords
region
sheet glass
plate
scribe line
glass
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2019185419A
Other languages
Japanese (ja)
Other versions
JP2021059476A (en
Inventor
力 岸田
拓也 塩路
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Electric Glass Co Ltd
Original Assignee
Nippon Electric Glass Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Electric Glass Co Ltd filed Critical Nippon Electric Glass Co Ltd
Priority to JP2019185419A priority Critical patent/JP7336071B2/en
Priority to PCT/JP2020/034941 priority patent/WO2021070579A1/en
Priority to KR1020227004507A priority patent/KR20220079515A/en
Priority to CN202080059179.1A priority patent/CN114302865A/en
Publication of JP2021059476A publication Critical patent/JP2021059476A/en
Application granted granted Critical
Publication of JP7336071B2 publication Critical patent/JP7336071B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、板ガラスをスクライブ線に沿って割断する技術を含む板ガラスの製造技術の改良に関する。 TECHNICAL FIELD The present invention relates to improvements in sheet glass manufacturing techniques, including techniques for cutting sheet glass along scribe lines.

周知のように、板ガラスは、液晶ディスプレイ、プラズマディスプレイ、有機ELディスプレイ等のディスプレイ用のガラス基板や、有機EL照明用のカバーガラスなどに代表されるように、各種分野に利用されている。この種の板ガラスを製造する際には、大型の板ガラスから小型の板ガラスを切り出す工程や、板ガラスの辺に沿う端部をトリミングする工程などが実行される。これらの工程では、通例、板ガラスにスクライブ線を形成した後、そのスクライブ線に沿って板ガラスを割断することが行われる。 As is well known, plate glass is used in various fields, typified by glass substrates for displays such as liquid crystal displays, plasma displays, and organic EL displays, and cover glasses for organic EL lighting. When manufacturing this type of plate glass, a step of cutting a small plate glass from a large plate glass, a step of trimming edges along the sides of the plate glass, and the like are performed. In these processes, usually, after forming a scribe line on the plate glass, the plate glass is cut along the scribe line.

この種の板ガラスを割断する方法の具体例としては、特許文献1に開示された方法が挙げられる。同文献に開示の方法では、板ガラスの表面にスクライブ線を形成した後、板ガラスの第1領域(スクライブ線の一方側の領域)の裏面を裏面支持部材で支持しておく。そして、この状態で、ローラ(転動体)が板ガラスの第2領域(スクライブ線の他方側の領域)の表面に沿って転動しながら第2領域を裏面側に押し込む。このローラによる押し込み動作により、スクライブ線の近傍に曲げ応力を作用させ、板ガラスをスクライブ線に沿って割断する。 A specific example of a method for breaking this type of sheet glass is the method disclosed in Patent Document 1. In the method disclosed in the document, after scribe lines are formed on the surface of the sheet glass, the back surface of the first area (area on one side of the scribe line) of the sheet glass is supported by a back support member. Then, in this state, the roller (rolling element) rolls along the surface of the second region (the region on the other side of the scribe line) of the plate glass and pushes the second region toward the back side. This pressing operation by the roller causes bending stress to act in the vicinity of the scribe line, thereby breaking the plate glass along the scribe line.

特開2017-226549号公報JP 2017-226549 A

ところで、特許文献1に開示のように、ローラを用いて板ガラスを割断しようとすると、ローラが板ガラスに点接触或いは線接触すること等に起因して、以下に示すような問題が生じる。 By the way, as disclosed in Patent Document 1, if a roller is used to break a plate glass, the following problems arise due to point contact or line contact of the roller with the plate glass.

すなわち、割断前の板ガラスには、反りが発生している場合がある。この反りを有する板ガラスをローラが裏面側に押し込んでいく際には、板ガラスのうちで反りに伴って張り出す部分にローラが点接触または線接触するため、ローラからの押し込み力が、板ガラスの第2領域に局所的に作用する。そのため、板ガラスのスクライブ線の近傍に曲げ応力を均等に作用させることができず、スクライブ線に沿った適正な割断が阻害される。その結果、板ガラスの割断部にチッピング(割断端面の不当なクラック)が発生して多量のガラス粉が飛散する等の不具合を招く。 That is, in some cases, sheet glass before breaking has warpage. When the roller pushes the warped sheet glass toward the back side, the roller comes into point contact or line contact with the portion of the sheet glass that protrudes due to the warp. It acts locally on two areas. Therefore, the bending stress cannot be uniformly applied in the vicinity of the scribe line of the plate glass, and proper cleaving along the scribe line is hindered. As a result, chipping (improper cracking of the cut end face) occurs at the cut portion of the sheet glass, causing problems such as scattering of a large amount of glass powder.

また、同文献の図4(b)に示されているように、ローラが板ガラスを裏面側に押し込んでいく際には、板ガラスの第2領域が全体に亘って湾曲変形する。この状態で、板ガラスのスクライブ線の近傍に十分な曲げ応力を作用させるためには、ローラの移動距離(図例の下方への移動距離)を長くして全体に亘って曲率の大きな湾曲変形を生じさせる必要がある。その結果、割断作業に要する時間の長期化や、ローラを移動させる機構の大型化等を招くおそれがある。 Further, as shown in FIG. 4(b) of the same document, when the roller pushes the sheet glass toward the rear surface side, the entire second region of the sheet glass is curved and deformed. In this state, in order to apply a sufficient bending stress to the vicinity of the scribe line of the plate glass, the moving distance of the roller (the downward moving distance in the figure) is increased to cause bending deformation with a large curvature over the entire surface. need to occur. As a result, there is a possibility that the time required for the cutting work will be prolonged, and the mechanism for moving the rollers will be enlarged.

以上の観点から、本発明は、割断時における板ガラスの裏面側への押し込み動作を良好に行えるようにして、板ガラスをスクライブ線に沿って適正に割断することを課題とする。 In view of the above, an object of the present invention is to properly cut the glass plate along the scribe line by enabling the operation of pushing the glass plate toward the back surface side during cutting.

上記課題を解決するために創案された本発明の第1の側面は、板ガラスの第1領域と第2領域との境界部の表面側にスクライブ線を形成し、前記スクライブ線に沿って前記板ガラスを割断する割断工程を含む板ガラスの製造方法において、前記割断工程では、裏面支持部材が前記第1領域の裏面を支持した状態にある時に、押し込み部材の平面部が前記第2領域の表面に接触した状態で回転しながら該第2領域を裏面側に押し込むことによって、前記スクライブ線に沿って前記板ガラスを割断することに特徴づけられる。なお、上記の板ガラスは、板厚が500μm以下であることが好ましく、板厚が300μm以下であることがより好ましい。また、この板ガラスは、可撓性を有していることが好ましい。 A first aspect of the present invention, which has been devised to solve the above problems, forms a scribe line on the surface side of a boundary between a first region and a second region of a sheet glass, and along the scribe line, the sheet glass In the method for manufacturing a plate glass, the flat portion of the pressing member contacts the surface of the second region when the back surface supporting member is in a state of supporting the back surface of the first region in the cutting step. The plate glass is cut along the scribe line by pressing the second region toward the rear surface side while rotating in this state. The sheet glass described above preferably has a thickness of 500 μm or less, and more preferably has a thickness of 300 μm or less. Moreover, it is preferable that this plate glass has flexibility.

この方法によれば、押し込み部材の平面部は、板ガラスの第2領域の表面が平面状をなす場合には当該表面に面接触し、また当該表面が凸部や凹部などを有する場合には当該表面に複数箇所で接触する。したがって、押し込み部材の平面部が、板ガラスの第2領域の表面に接触した状態で回転しながら該第2領域を裏面側に押し込む際には、両者の接触面積が広くなる。そのため、ガラス板に反りが発生していても、押し込み部材の平面部から第2領域に作用する押し込み力が分散され、板ガラスの反りが矯正されると共に、押し込み力が局所的に作用し難くなる。これにより、スクライブ線の近傍には、均等に曲げ応力が作用し、板ガラスを適正に割断することが可能となる。その結果、板ガラスの割断部にチッピングが発生して多量のガラス粉が飛散する等の不具合が回避される。この場合、板ガラスの反りは、板ガラスの表面におけるスクライブ線及びこれと平行な任意の仮想直線が湾曲するような反りであれば特に有効である。また、この方法によれば、押し込み部材の平面部が第2領域を裏面側に押し込んだ際には、押し込み領域が広い範囲で平面状になるために、第2領域が全体に亘って湾曲変形せずに、第2領域における当該平面部との接触部位及びその接触部位からスクライブ線に至るまでの部位が平坦な形状に近い形状になる。これにより、第2領域のスクライブ線の近傍が、屈曲形状に近い形状つまり大きな曲率で湾曲した形状になり、十分な曲げ応力が作用するため、押し込み部材が裏側に向かって短い距離を移動するだけで、板ガラスの割断を完了することができる。これによっても、板ガラスをスクライブ線に沿って適正に割断することができると共に、割断作業に要する時間の短縮や、押し込み部材を移動させる機構のコンパクト化等が実現する。 According to this method, the planar portion of the pressing member is in surface contact with the surface of the second region of the sheet glass when the surface is planar, and when the surface has protrusions or recesses, Multiple points of contact with the surface. Therefore, when the planar portion of the pressing member rotates while being in contact with the surface of the second region of the plate glass and presses the second region toward the back side, the contact area between the two is increased. Therefore, even if the glass sheet is warped, the pressing force acting from the flat portion of the pressing member to the second region is dispersed, the warp of the plate glass is corrected, and the pressing force is less likely to act locally. . As a result, a bending stress acts evenly in the vicinity of the scribe line, and the plate glass can be properly cleaved. As a result, problems such as chipping occurring at the cut portion of the plate glass and scattering of a large amount of glass powder can be avoided. In this case, the warpage of the sheet glass is particularly effective if the scribe line on the surface of the sheet glass and any imaginary straight line parallel thereto are curved. Further, according to this method, when the flat portion of the pushing member pushes the second region toward the rear surface side, the pushing region becomes flat over a wide range, so that the second region is curved and deformed as a whole. Therefore, the contact portion with the flat portion in the second region and the portion from the contact portion to the scribe line have a nearly flat shape. As a result, the vicinity of the scribe line of the second region becomes a shape close to a bent shape, that is, a shape curved with a large curvature, and sufficient bending stress acts, so that the pushing member only moves a short distance toward the back side. , the breaking of the sheet glass can be completed. In this way, the sheet glass can be properly cut along the scribe line, and the time required for the cutting work can be shortened, and the mechanism for moving the pressing member can be made compact.

この方法において、前記平面部は、前記スクライブ線に沿う方向に延びる軸線の廻りに回転することが好ましい。ここで、上記の「スクライブ線に沿う方向に延びる軸線」とは、板ガラスに反りが発生していない状態で形成されるスクライブ線に沿う方向に延びる軸線を意味する(以下、同様)。 In this method, the planar portion preferably rotates around an axis extending along the scribe line. Here, the above-mentioned "axis extending in the direction along the scribe line" means an axis extending in the direction along the scribe line formed in a state in which the sheet glass is not warped (the same applies hereinafter).

このようにすれば、押し込み部材の平面部が第2領域の表面に接触した状態をそのまま維持して、当該平面部を適正に回転させていくことができる。詳述すると、当該平面部の回転中心である軸線が、スクライブ線に沿って延びていない場合には、当該平面部と第2領域との接触状態が偏るなどして、第2領域の表面に傷が付いたり或いはスクライブ線の近傍に曲げ応力が偏って作用したりするおそれがある。しかし、ここでの構成によれば、このような不具合が適切に回避される。 In this way, the flat portion of the pushing member can be properly rotated while maintaining the state in which the flat portion is in contact with the surface of the second region. More specifically, if the axis line that is the center of rotation of the flat portion does not extend along the scribe line, the contact state between the flat portion and the second region will be biased, and the surface of the second region will be affected. There is a risk that it will be scratched or that bending stress will act unevenly in the vicinity of the scribe line. However, according to the configuration here, such problems are appropriately avoided.

この方法において、前記軸線は、前記平面部が前記第2領域を裏面側に押し込む方向に平行移動するようにしてもよい。 In this method, the axis may be moved in parallel in a direction in which the planar portion pushes the second region toward the back side.

このようにすれば、簡単な構成により、押し込み部材の平面部を第2領域の表面に接触させた状態をそのまま維持しつつ、より一層適正に当該平面部を回転させていくことができる。 In this way, with a simple configuration, the flat portion of the pushing member can be rotated more appropriately while maintaining the state in which the flat portion is in contact with the surface of the second region.

この方法において、前記平面部が前記第2領域を裏面側に押し込むことに伴う前記第2領域の前記平面部との接触部位の角度変化に追随して、前記平面部の角度が変化するようにしてもよい。 In this method, the angle of the flat portion is changed in accordance with the change in the angle of the contact portion of the second region with the flat portion as the flat portion pushes the second region toward the rear surface side. may

このようにすれば、押し込み部材の平面部が第2領域を裏面側に押し込んでいく際に、第2領域における当該平面部との接触部位の角度(傾斜角度)が変化しても、当該平面部の角度は、変化する第2領域の角度に倣うことになる。これにより、押し込み部材と第2領域との接触状態を、常に好適な状態に維持することができる。 With this configuration, when the flat portion of the pushing member pushes the second region toward the rear surface side, even if the angle (inclination angle) of the contact portion of the second region with the flat portion changes, the plane The angle of the part will follow the angle of the second region which changes. As a result, the contact state between the pushing member and the second region can always be maintained in a favorable state.

以上の方法において、前記割断工程では、前記板ガラスを、前記スクライブ線が上下方向を向くように吊り下げ支持するようにしてもよい。 In the above method, in the cutting step, the plate glass may be suspended and supported so that the scribe lines are oriented vertically.

このようにすれば、板ガラスに反りが発生している場合の既述の作用効果を顕著に得ることができる。詳述すると、板ガラスを定盤等の上に平置き姿勢で載置して割断する場合には、板ガラスの反りが小さくなるが、ここでの構成のように板ガラスを吊り下げ支持した場合には、反りが大きくなる。このような場合でも、板ガラスの反りに対しては、既述のように適正に対処可能であるため、その作用効果が格別なものになる。 By doing so, it is possible to remarkably obtain the effects described above when the sheet glass is warped. More specifically, when the plate glass is laid flat on a surface plate or the like and cut, the warpage of the plate glass is reduced. , the warpage increases. Even in such a case, since the warp of the plate glass can be properly dealt with as described above, the effect is exceptional.

以上の方法において、前記割断工程では、前記第2領域の裏面を吸着保持するようにしてもよい。 In the above method, in the cutting step, the back surface of the second region may be held by suction.

このようにすれば、第2領域の裏面の吸着保持によって、板ガラスの反りを補助的に小さくすることができるため、より一層確実にスクライブ線の近傍に均等な曲げ応力を作用させることができる。また、割断後においては、第1領域から分離した第2領域が継続して吸着保持されるため、第2領域を落下させずに退避位置まで搬送して、円滑に廃棄処分や回収処理等を行うことができる。 In this way, the back surface of the second region is sucked and held, so that the warp of the sheet glass can be supplementarily reduced, so that a uniform bending stress can be applied to the vicinity of the scribe line more reliably. In addition, after cutting, the second area separated from the first area is continuously held by suction, so that the second area is transported to the retracted position without dropping, and disposal and recovery processing can be performed smoothly. It can be carried out.

以上の方法において、前記平面部は、前記第2領域の前記スクライブ線と対向する端縁部を含む部位の表面に接触するようにしてもよい。 In the above method, the planar portion may be in contact with the surface of the portion including the edge portion facing the scribe line of the second region.

このようにすれば、特許文献1に開示のようにローラを用いて板ガラスを割断する場合に、当該端縁部にローラが接触することにより生じる不具合を回避することができる。すなわち、板ガラスの当該端縁部(耳部と呼称されている部位)は、板ガラスの中央側の部位よりも厚肉であり且つ表面に凹凸が形成されている。そのため、当該端縁部にローラが点接触または線接触した状態で第2領域を押し込んだ場合には、当該端縁部とローラとの接触状態が押し込み位置に応じて変動するおそれがあり、これに伴い両者間にガタツキが生じて、割断を適正に行えなくなり得る。これに対して、平面部が当該端縁部に接触した状態で第2領域を押し込んでも、平面部と当該端縁部との接触状態は変動し難いため、両者間にガタツキが生じ難くなり、割断を良好に行うことができる。また、これによって、第2領域のスクライブ線と直交する幅方向寸法が狭い場合であっても、平面部が当該端縁部に接触した状態で良好に割断を行うことができる。 By doing so, it is possible to avoid problems caused by the roller coming into contact with the edge portion when breaking the plate glass using the roller as disclosed in Patent Document 1. That is, the edges of the plate glass (parts called lugs) are thicker than the central part of the plate glass and have unevenness on the surface. Therefore, when the second region is pushed in with the roller in point contact or line contact with the edge, the contact state between the edge and the roller may vary depending on the pressing position. As a result, rattling occurs between the two, and it may become impossible to properly perform cutting. On the other hand, even if the second region is pushed in while the flat portion is in contact with the edge portion, the contact state between the flat portion and the edge portion is unlikely to change, so that rattling between the two is less likely to occur. Cleavage can be performed well. Further, as a result, even when the dimension in the width direction perpendicular to the scribe line of the second region is narrow, it is possible to satisfactorily cut the sheet while the plane portion is in contact with the edge portion.

以上の方法において、前記押し込み部材は、板厚方向で対向する二つの表面のうちの一方の表面が前記平面部とされた板状部材であって、前記板状部材は、前記スクライブ線に沿う方向に延びる軸線の廻りに回転可能なローラを有するローラ付き部材に着脱可能に保持されていてもよい。 In the above method, the pressing member is a plate-like member having one of two surfaces facing each other in the plate thickness direction as the flat portion, and the plate-like member is along the scribe line It may be detachably held by a roller-equipped member having a roller rotatable about an axis extending in the direction.

このようにすれば、板ガラスの反りの程度に応じて、板状部材による第2領域の押し込みと、ローラによる第2領域の押し込みとを使い分けることができる。詳述すると、板ガラスの反りが割断に悪影響を及ぼすおそれがある場合には、板状部材によって第2領域を押し込むようにする。これに対して、板ガラスの反りが問題にならない程度である場合には、ローラ付き部材から板状部材を取り外して、ローラによって第2領域を押し込むようにする。これにより、板状部材により押し込みを行う場合の既述の利点と、ローラにより押し込みを行う場合の利点とを、兼ね備えることができる。なお、反りが問題にならない程度の板ガラスについて、ローラにより押し込みを行う場合の利点としては、押し込み時に第2領域の表面に傷が付き難くなる事やローラを移動させる機構の構成が簡素化される事などが挙げられる。 In this way, depending on the degree of warpage of the plate glass, pressing of the second region by the plate member and pressing of the second region by the roller can be selectively used. More specifically, if the warp of the plate glass may adversely affect the breaking, the plate-like member is pushed into the second region. On the other hand, if the warpage of the sheet glass is not a problem, the plate-shaped member is removed from the member with rollers, and the second region is pushed by the rollers. As a result, it is possible to combine the above-described advantage of pressing with a plate-like member and the advantage of pressing with a roller. The advantages of pushing in the sheet glass with rollers to such an extent that warpage is not a problem are that the surface of the second region is less likely to be damaged during pushing and the structure of the mechanism for moving the rollers is simplified. things, etc.

上記課題を解決するために創案された本発明の第2の側面は、第1領域と第2領域との境界部の表面側にスクライブ線が形成された板ガラスを、前記スクライブ線に沿って割断する割断装置を備えた板ガラスの製造装置において、前記割断装置は、前記第1領域の裏面を支持する裏面支持部材と、前記スクライブ線に沿って前記板ガラスを割断するために、前記第2領域の表面に接触した状態で回転しながら該第2領域を裏面側に押し込む平面部が形成された押し込み部材とを備えていることに特徴づけられる。 A second aspect of the present invention, which has been devised to solve the above-mentioned problems, is to cut a plate glass having a scribe line formed on the surface side of the boundary between the first region and the second region along the scribe line. In the plate glass manufacturing apparatus provided with a cutting device that performs the cutting, the cutting device includes a back surface support member that supports the back surface of the first region, and a second region for cutting the plate glass along the scribe line. A pressing member having a flat portion for pressing the second region toward the back side while rotating in contact with the front surface is provided.

この製造装置によれば、既述の製造方法の場合と同様にして、板ガラスの割断が適正に行われ、割断時のチッピングの発生や多量のガラス粉の飛散等が回避されると共に、割断に要する作業時間の短縮や押し込み部材を移動させる機構のコンパクト化等が実現する。 According to this manufacturing apparatus, in the same manner as in the manufacturing method described above, the sheet glass is properly cut, and the occurrence of chipping at the time of cutting and the scattering of a large amount of glass powder are avoided. It is possible to shorten the work time required and to make the mechanism for moving the pressing member compact.

本発明によれば、割断時における板ガラスの裏面側への押し込み動作が良好に行われて、板ガラスがスクライブ線に沿って適正に割断される。 ADVANTAGE OF THE INVENTION According to this invention, the operation|movement which pushes in to the back surface side of plate glass at the time of breaking is performed favorably, and plate glass is broken appropriately along a scribe line.

本発明の実施形態に係る板ガラスの製造装置に含まれる割断装置を示す斜視図である。1 is a perspective view showing a breaking device included in a sheet glass manufacturing apparatus according to an embodiment of the present invention. FIG. 図2(a)、(b)は、本発明の実施形態に係る板ガラスの製造装置に含まれる割断装置の要部を下方から視た拡大概略下面図である。FIGS. 2(a) and 2(b) are enlarged schematic bottom views of main parts of the breaking device included in the sheet glass manufacturing apparatus according to the embodiment of the present invention, as viewed from below. 図3(a)は、本発明の実施形態に係る板ガラスの製造装置に含まれる割断装置を側方から視た概略側面図であり、図3(b)は、本発明の一実施形態に係る板ガラスの製造装置に含まれる割断装置の要部を下方から視た拡大概略下面図である。FIG. 3(a) is a schematic side view of a breaking device included in a sheet glass manufacturing apparatus according to an embodiment of the present invention, and FIG. Fig. 2 is an enlarged schematic bottom view of a main part of a cutting device included in the plate glass manufacturing apparatus, as viewed from below; 図4(a)、(b)、(c)は、本発明の実施形態に係る板ガラスの製造方法に含まれる割断工程を示す概略下面図である。FIGS. 4(a), (b), and (c) are schematic bottom views showing the cutting step included in the method for manufacturing sheet glass according to the embodiment of the present invention. 図5(a)、(b)は、本発明の実施形態に係る板ガラスの製造方法に含まれる割断工程の第1の変形例を示す概略下面図である。FIGS. 5(a) and 5(b) are schematic bottom views showing a first modification of the cutting step included in the method for manufacturing sheet glass according to the embodiment of the present invention. 本発明の実施形態に係る板ガラスの製造方法に含まれる割断工程の第2の変形例を示す概略下面図である。It is a schematic bottom view which shows the 2nd modification of the cutting process included in the manufacturing method of the sheet glass which concerns on embodiment of this invention. 本発明の実施形態に係る板ガラスの製造方法に含まれる割断工程の第3の変形例を示す概略下面図である。It is a schematic bottom view which shows the 3rd modification of the cutting process included in the manufacturing method of the sheet glass which concerns on embodiment of this invention. 本発明の実施形態に係る板ガラスの製造方法に含まれる割断工程の第4の変形例を示す概略下面図である。It is a schematic bottom view which shows the 4th modification of the cutting process included in the manufacturing method of the sheet glass which concerns on embodiment of this invention.

以下、本発明の実施形態に係る板ガラスの製造方法及び製造装置について添付図面を参照しつつ説明する。 DESCRIPTION OF THE PREFERRED EMBODIMENTS A method and apparatus for manufacturing plate glass according to embodiments of the present invention will be described below with reference to the accompanying drawings.

図1は、本発明の一実施形態に係る板ガラスの製造装置に含まれる割断装置1を例示する斜視図である。同図に示すように、板ガラスGは、表面側(符号Ga、Gxの側)に形成されたスクライブ線Sを境界として、その幅方向一方側(矢印A方向側)が第1領域G1とされ、その幅方向他方側(矢印B方向側)が第2領域G2とされる。この実施形態では、第1領域G1が製品部分となり、第2領域G2が非製品部分となる。ただし、第1領域G1と第2領域G2の双方が製品部分となってもよい。図例では、スクライブ線Sは、板ガラスGの上端及び下端に到達していないが、上端及び下端に到達していてもよい。 FIG. 1 is a perspective view illustrating a breaking device 1 included in a plate glass manufacturing apparatus according to an embodiment of the present invention. As shown in the figure, the sheet glass G has a first region G1 on one side in the width direction (the side in the direction of the arrow A) with a scribe line S formed on the surface side (the side of the symbols Ga and Gx) as a boundary. , the other side in the width direction (the arrow B direction side) is a second region G2. In this embodiment, the first area G1 is the product portion and the second area G2 is the non-product portion. However, both the first area G1 and the second area G2 may be part of the product. In the illustrated example, the scribe line S does not reach the upper and lower ends of the plate glass G, but may reach the upper and lower ends.

板ガラスGは、スクライブ線Sが上下方向を向くように吊り下げ支持されている。板ガラスGの板厚は、例えば200~2000μmとすることができる。板厚が小さいほど反りが発生し易くなると共に発生する反りが大きくなり、後述の本発明の反りを矯正する効果が顕著となるので、板厚は、500μm以下が好ましく、より好ましくは300μm以下である。また、板ガラスGは、可撓性を有していることが好ましい。この実施形態では、板ガラスGに反りが発生している。この反りは、板ガラスGの表面におけるスクライブ線S及びこれと平行な任意の仮想直線が湾曲する形状を呈している。 The plate glass G is suspended and supported so that the scribe line S is oriented in the vertical direction. The plate thickness of the plate glass G can be, for example, 200 to 2000 μm. The smaller the plate thickness, the more easily warpage occurs and the larger the warpage that occurs, and the effect of correcting warpage of the present invention, which will be described later, becomes remarkable. be. Moreover, it is preferable that the plate glass G has flexibility. In this embodiment, the sheet glass G is warped. This warp has a shape in which the scribe line S on the surface of the plate glass G and any imaginary straight line parallel thereto are curved.

割断装置1は、板ガラスGを曲げ応力によってスクライブ線Sに沿って割断するものである。詳述すると、割断装置1は、板ガラスGを吊り下げ支持する把持機構2と、第1領域G1の裏面Gb側を支持する裏面支持部材3と、第2領域G2の裏面Gy側を吸着保持する吸着機構4と、第2領域G2の表面Gxに接触した状態で矢印C方向に回転しながら第2領域G2を裏面Gy側に押し込む押し込み部材5とを備えている。この実施形態では、押し込み部材5は、板厚方向で対向する2つの表面のうちの一方の表面が、第2領域G2の表面Gxに接触する平面部5aとされた板状部材である(図2(b)参照)。 The breaking device 1 breaks a plate glass G along a scribe line S by bending stress. More specifically, the breaking device 1 includes a gripping mechanism 2 that suspends and supports the plate glass G, a back surface support member 3 that supports the back surface Gb side of the first region G1, and a back surface Gy side of the second region G2 that is held by suction. It has a suction mechanism 4 and a pushing member 5 that pushes the second region G2 toward the rear surface Gy side while rotating in the direction of arrow C while being in contact with the front surface Gx of the second region G2. In this embodiment, the pushing member 5 is a plate-like member having two surfaces facing each other in the plate thickness direction, one of which is a flat portion 5a that contacts the surface Gx of the second region G2 (Fig. 2(b)).

把持機構2は、第1領域G1の上端部を把持した状態で、板ガラスGを幅方向に移動させるものである。なお、把持機構2は、板ガラスGの上方を幅方向に沿って延びるレール(図示略)にスライド可能に保持されている。板ガラスGを割断する工程が行われる際には、把持機構2及び板ガラスGは停止した状態になる。また、把持機構2は、第1領域G1の上端部における幅方向の複数箇所に配置してもよい。 The gripping mechanism 2 moves the plate glass G in the width direction while gripping the upper end of the first region G1. The gripping mechanism 2 is slidably held by a rail (not shown) extending in the width direction above the plate glass G. As shown in FIG. When the step of breaking the plate glass G is performed, the gripping mechanism 2 and the plate glass G are stopped. Moreover, the gripping mechanism 2 may be arranged at a plurality of locations in the width direction in the upper end portion of the first region G1.

裏面支持部材3は、第1領域G1のスクライブ線S側の端部における裏面Gb側に配置されている。裏面支持部材3とスクライブ線Sとの幅方向の離間距離L1は、例えば10~30mmであり、好ましくは10~20mmである(図4(a)参照)。この実施形態では、裏面支持部材3は、第1領域G1の裏面Gbを支持する支持面が平面とされ且つ上下方向に長尺な柱状体または板状体(定盤)である。なお、裏面支持部材3の形状は、丸棒状などであってもよい。また、裏面支持部材3は、第1領域G1の上端Gd及び下端Geから上下に食み出しているが、上端Gd及び下端Geに到達しない長さであってもよい。 The back surface support member 3 is arranged on the back surface Gb side at the end portion on the scribe line S side of the first region G1. A distance L1 between the back support member 3 and the scribe line S in the width direction is, for example, 10 to 30 mm, preferably 10 to 20 mm (see FIG. 4A). In this embodiment, the back surface supporting member 3 is a columnar body or a plate-like body (surface plate) having a flat support surface for supporting the back surface Gb of the first region G1 and elongated in the vertical direction. In addition, the shape of the back support member 3 may be a round bar shape or the like. Further, the back support member 3 protrudes vertically from the upper end Gd and the lower end Ge of the first region G1, but the length may be such that it does not reach the upper end Gd and the lower end Ge.

吸着機構4は、上下方向に長尺な保持基材6と、保持基材6の長手方向に等間隔で装着された複数個(図例では5個)の吸着パッド7とを備えている。保持基材6は、ロボットアーム等の駆動手段(図示略)の動作によって移動する構成とされている。また、吸着パッド7は、伸縮可能なゴムや樹脂等の弾性部材で形成され、第2領域G2の裏面Gyを負圧により吸着するものである。 The suction mechanism 4 includes a vertically elongated holding base 6 and a plurality of (five in the figure) suction pads 7 mounted at equal intervals in the longitudinal direction of the holding base 6 . The holding base 6 is configured to be moved by the operation of driving means (not shown) such as a robot arm. The suction pad 7 is made of an elastic member such as elastic rubber or resin, and suctions the back surface Gy of the second region G2 with negative pressure.

押し込み部材としての板状部材5は、第2領域G2の表面Gx側に配置されている。板状部材5とスクライブ線Sとの幅方向の離間距離L2は、例えば80~160mmである(図4(a)参照)。なお、ここでいう離間距離L2は、第2領域G2を押し込む前の離間距離である。この実施形態では、板状部材5は、上下方向に長尺な平板であって、第2領域G2の上端Gf及び下端Ggから上下に食み出しているが、上端Gf及び下端Ggに到達しない長さであってもよい。 The plate member 5 as a pushing member is arranged on the surface Gx side of the second region G2. A widthwise distance L2 between the plate member 5 and the scribe line S is, for example, 80 to 160 mm (see FIG. 4A). The separation distance L2 here is the separation distance before the second region G2 is pushed. In this embodiment, the plate-like member 5 is a flat plate elongated in the vertical direction, and protrudes vertically from the upper end Gf and the lower end Gg of the second region G2, but does not reach the upper end Gf and the lower end Gg. It can be length.

板状部材5の表側には、板状部材5を着脱可能に保持するローラ付き部材8が配設されている。このローラ付き部材8は、スクライブ線Sに沿う方向に延びるローラ軸9と、ローラ軸9の軸方向に等間隔で配列された複数個(図例では5個)のローラ10と、ローラ軸9を支持する支持体11とを備えている。なお、ここでいうスクライブ線Sは、板ガラスGに反りが全く無いとした場合のスクライブ線である。この実施形態では、板状部材5は、結束バンド12を用いてローラ軸9に連結されている。結束バンド12は、板状部材5とローラ軸9とに跨って巻き付け及び巻き外しが可能とされ、これにより板状部材5がローラ付き部材8に着脱可能とされている。支持体11は、ロボットアーム等の駆動手段(図示略)の動作によって移動する構成とされ、これによりローラ付き部材8と板状部材5とが同期して移動するようになっている。 A member 8 with rollers is arranged on the front side of the plate-like member 5 to detachably hold the plate-like member 5 . The roller-equipped member 8 includes a roller shaft 9 extending in a direction along the scribe line S, a plurality of rollers 10 (five in the example shown) arranged at equal intervals in the axial direction of the roller shaft 9 , the roller shaft 9 and a support 11 for supporting the The scribe line S referred to here is a scribe line when the sheet glass G is not warped at all. In this embodiment, the plate member 5 is connected to the roller shaft 9 using a binding band 12 . The binding band 12 can be wound around and unwound across the plate-like member 5 and the roller shaft 9 , so that the plate-like member 5 can be attached to and detached from the member 8 with rollers. The support 11 is configured to be moved by the operation of driving means (not shown) such as a robot arm, so that the roller-equipped member 8 and the plate-like member 5 are moved synchronously.

図2(a)、(b)は、板状部材5の周辺を下方から視た下面図である。図2(a)に示すように、各ローラ10は、板状部材5における平面部5aと対向する表面(平面状をなす)に接触して、板状部材5を押圧するものである。板状部材5は、同図に鎖線で示すように、各ローラ10と同一箇所で接触した状態を維持して、ローラ軸9の廻りに回転する構成とされている。したがって、板状部材5から表側に離間した位置に、板状部材5の平面部5aの回転中心となるローラ軸9(厳密には、ローラ軸9の中心である軸線9a)が存在している。ローラ軸9の軸線9aと板状部材5との離間距離L3(ローラ10の半径)は、例えば10~30mmである。 2A and 2B are bottom views of the periphery of the plate member 5 viewed from below. As shown in FIG. 2( a ), each roller 10 presses the plate-like member 5 by contacting the surface (having a flat surface) facing the flat portion 5 a of the plate-like member 5 . The plate-like member 5 is configured to rotate around the roller shaft 9 while maintaining contact with the rollers 10 at the same location, as indicated by the dashed line in FIG. Therefore, the roller shaft 9 (strictly speaking, the axis 9a that is the center of the roller shaft 9) that serves as the center of rotation of the planar portion 5a of the plate-like member 5 is present at a position spaced from the plate-like member 5 toward the front side. . A distance L3 (the radius of the roller 10) between the axis 9a of the roller shaft 9 and the plate member 5 is, for example, 10 to 30 mm.

図2(b)に示すように、板状部材5は、ローラ10に接触した状態を維持して、裏側へのD方向に直進移動する構成とされている。このD方向は、第2領域G2の表面Gxと直交する方向である。ここでいう第2領域G2の表面Gxとは、反りが全く無いとした場合の第2領域G2の折割工程前の表面Gxである。同図に鎖線で示すように、ローラ10がD方向に直進移動した場合には、第2領域G2の角度変化に追随して、板状部材5の平面部5aの角度が変化する。ここで、ローラ軸9(軸線9a)の移動経路Zを基準にすれば、板状部材5の平面部5aは、角度変化と共に、スクライブ線Sに近づく側に距離L6だけ相対移動する。したがって、当該平面部5aと第2領域G2との接触位置も、ローラ軸9の移動経路Zに対して、スクライブ線Sに近づく側に距離L6だけ相対移動する。この場合、仮に特許文献1に開示のようにローラ10が第2領域G2の表面Gxに直接接触していたならば、ローラ10と第2領域G2との接触位置aは、上記の距離L6よりも短い距離L7だけスクライブ線Sに近づく側に相対移動する。 As shown in FIG. 2(b), the plate-like member 5 is configured to keep contact with the roller 10 and move straight in the D direction toward the back side. This D direction is a direction perpendicular to the surface Gx of the second region G2. The surface Gx of the second region G2 referred to here is the surface Gx of the second region G2 before the folding/breaking process, assuming that there is no warpage. As indicated by the dashed line in the figure, when the roller 10 moves straight in the direction D, the angle of the planar portion 5a of the plate-like member 5 changes following the angle change of the second region G2. Here, if the movement path Z of the roller shaft 9 (axis line 9a) is used as a reference, the planar portion 5a of the plate-like member 5 relatively moves toward the scribe line S by a distance L6 as the angle changes. Therefore, the contact position between the flat portion 5a and the second region G2 also moves relative to the movement path Z of the roller shaft 9 toward the scribe line S by a distance L6. In this case, if the roller 10 were in direct contact with the surface Gx of the second region G2 as disclosed in Patent Document 1, the contact position a between the roller 10 and the second region G2 would be less than the distance L6. relative movement toward the scribe line S by a short distance L7.

板状部材5の平面部5aは、第2領域G2の表面Gxに傷が付き難い材質で形成されている。したがって、当該平面部5aは、樹脂等で形成されることが好ましい。さらに、板状部材5は、適度な可撓性を有していることが好ましい。詳しくは、板状部材5は、板ガラスGと同程度またはそれよりも高い剛性を備えた上で可撓性を有していることが好ましい。これらの観点から、板状部材5は、プラスチック段ボールやパロニアに代表される多孔質樹脂板または発泡樹脂板等であることが好ましい。 The planar portion 5a of the plate member 5 is made of a material that does not easily scratch the surface Gx of the second region G2. Therefore, the flat portion 5a is preferably made of resin or the like. Furthermore, it is preferable that the plate-like member 5 has moderate flexibility. More specifically, it is preferable that the plate member 5 has rigidity equal to or higher than that of the plate glass G and has flexibility. From these points of view, the plate-like member 5 is preferably a porous resin plate or foamed resin plate represented by plastic corrugated cardboard or paronia.

次に、以上のように構成された製造装置を用いた板ガラスの製造方法を説明する。 Next, a method for manufacturing sheet glass using the manufacturing apparatus configured as described above will be described.

まず、図1に示す位置の上流側の工程において、板ガラスGを把持機構2により吊り下げ支持した状態で、ホイールカッターによる押圧やレーザーの照射等により、板ガラスGの表面Gxにスクライブ線Sを形成する。次に、スクライブ線Sが形成された板ガラスGを把持機構2で吊り下げ支持した状態のまま、板ガラスGを幅方向に搬送して停止させる。板ガラスGが停止した時点で、図1に示すように、裏面支持部材3が表側に向かって移動して板ガラスGの第1領域G1の裏面Gyに接触する。また、ローラ付き部材8が裏側に向かって移動することで、板状部材5の平面部5aが第2領域G2の表面Gxに接触する。さらに、吸着機構4の保持基材6が表側に向かって移動することで、吸着パッド7が第2領域G2の裏面Gyを吸着する。 First, in a process on the upstream side of the position shown in FIG. 1, a scribe line S is formed on the surface Gx of the sheet glass G by pressing with a wheel cutter, laser irradiation, or the like while the sheet glass G is suspended and supported by the gripping mechanism 2. do. Next, while the sheet glass G on which the scribe line S is formed is suspended and supported by the gripping mechanism 2, the sheet glass G is conveyed in the width direction and stopped. When the sheet glass G stops, the back support member 3 moves toward the front side and contacts the back surface Gy of the first region G1 of the sheet glass G, as shown in FIG. Further, the planar portion 5a of the plate member 5 comes into contact with the surface Gx of the second region G2 by moving the member 8 with the roller toward the back side. Furthermore, as the holding base material 6 of the adsorption mechanism 4 moves toward the front side, the adsorption pad 7 adsorbs the back surface Gy of the second region G2.

そして、板状部材5の平面部5aは、第2領域G2の表面Gxに面接触した状態を維持して、第2領域G2を裏面Gy側に押し込んでいく。この段階で、第2領域G2と板状部材5の平面部5aとの面接触部Gw周辺は、図3(a)に示す側面視及び図3(b)に示す下面視(実線で描かれた態様)において、反りが殆ど無い平坦な形状になる。この場合、仮に特許文献1に開示のようにローラ10を第2領域G2の表面Gxに直接接触させたならば、例えば、図3(b)に鎖線で示すように、ローラ10が板ガラスGのうちで反りに伴って張り出した部分に点接触または線接触することで、第2領域G2のローラ10との接触部bの近傍が局所的に大きく窪む。そして、この局所的な窪みは、第2領域G2の広い範囲に不当な変形を生じさせる要因になる。そのため、板ガラスGの割断時には、スクライブ線Sの近傍に均等な曲げ応力が生じ難くなる。これに対して、板状部材5の平面部5aが第2領域G2の表面Gxに面接触していれば、第2領域G2と当該平面部5aとの面接触部Gw周辺が平坦な形状になることから、第2領域G2の広い範囲に不当な変形を生じさせるには至らない。これにより、板ガラスGの割断時には、特許文献1に開示の場合と比較して、スクライブ線Sの近傍に均等に曲げ応力が作用し、チッピングの発生や多量のガラス粉の飛散等が生じ難くなる。なお、第2領域G2の裏面Gyは、吸着パッド7により吸着保持されているため、板ガラスGの反りをより一層小さくする効果が得られる。ただし、吸着パッド7は、伸縮する等の容易に変形する特性を有しているため、吸着パッド7のみでは板ガラスGの反りを十分に小さくすることができず、反りの低減について補助的な役割を果たす。 Then, the planar portion 5a of the plate-like member 5 is kept in surface contact with the surface Gx of the second region G2, and pushes the second region G2 toward the rear surface Gy. At this stage, the periphery of the surface contact portion Gw between the second region G2 and the planar portion 5a of the plate member 5 is shown in the side view shown in FIG. 3(a) and the bottom view shown in FIG. ), the flat shape is obtained with almost no warpage. In this case, if the roller 10 is brought into direct contact with the surface Gx of the second region G2 as disclosed in Patent Document 1, for example, as shown by the chain line in FIG. By making point contact or line contact with the portion that protrudes due to the warpage, the vicinity of the contact portion b with the roller 10 in the second region G2 is locally greatly depressed. Then, this local depression becomes a factor that causes unreasonable deformation in a wide range of the second region G2. Therefore, uniform bending stress is less likely to occur in the vicinity of the scribe line S when the plate glass G is broken. On the other hand, if the plane portion 5a of the plate member 5 is in surface contact with the surface Gx of the second region G2, the periphery of the plane contact portion Gw between the second region G2 and the plane portion 5a becomes flat. Therefore, it does not result in unreasonable deformation in a wide range of the second region G2. As a result, when the sheet glass G is broken, compared with the case disclosed in Patent Document 1, the bending stress acts evenly in the vicinity of the scribe line S, and chipping and scattering of a large amount of glass powder are less likely to occur. . In addition, since the rear surface Gy of the second region G2 is suction-held by the suction pad 7, the effect of further reducing the warpage of the plate glass G can be obtained. However, since the suction pad 7 has a characteristic of being easily deformed such as to expand and contract, the suction pad 7 alone cannot sufficiently reduce the warpage of the plate glass G, and the suction pad 7 plays an auxiliary role in reducing the warpage. fulfill

図4(a)~(c)は、板状部材5の平面部5aが回転しながら第2領域G2を裏面Gy側に押し込み、板ガラスGを割断していく工程を時系列で例示している。まず、図4(a)に示すように、ローラ付き部材8を移動させて、板状部材5の平面部5aを第2領域G2の表面Gxに面接触させる。このとき、ローラ10は板状部材5に接触した状態にあり、板状部材5及び保持基材6は双方共に傾斜しない状態(第1領域G1の表面Gaと平行な状態)にある。以下、この状態を初期状態とよぶ。 FIGS. 4(a) to 4(c) exemplify steps in chronological order in which the flat portion 5a of the plate member 5 rotates and pushes the second region G2 toward the rear surface Gy to cut the plate glass G. . First, as shown in FIG. 4A, the member 8 with rollers is moved to bring the planar portion 5a of the plate member 5 into surface contact with the surface Gx of the second region G2. At this time, the roller 10 is in contact with the plate-like member 5, and both the plate-like member 5 and the holding base 6 are in a non-tilted state (parallel to the surface Ga of the first region G1). This state is hereinafter referred to as an initial state.

次に、図4(b)に示すように、ローラ10及びローラ軸9がD方向に直進移動(平行移動)することで、板状部材5の平面部5aは、第2領域G2の表面Gxに面接触した状態を維持してローラ軸9(軸線9a)の廻りに回転する。これにより、板ガラスGは裏面支持部材3を起点として撓む。このとき、板状部材5の平面部5aは、第2領域G2の表面Gxの角度変化に追随して、角度が変化する。そして、この過程では、第2領域G2における板状部材5の平面部5aとの面接触部Gwからスクライブ線Sに至るまでの部位が平坦に近い形状になるため、第2領域G2のスクライブ線Sの近傍は屈曲に近い形状つまり大きい曲率で湾曲した形状になる。ここで、同図に鎖線で示す湾曲線Wは、特許文献1に開示のようにローラ10が第2領域G2の表面Gxに直接接触していたとした場合に、第2領域G2の表面Gxが撓んだときの形状を描いたものである。この湾曲線Wは、第2領域G2のスクライブ線Sの近傍が小さい曲率で湾曲している。そのため、ローラ10が直接接触する場合よりも板状部材5の平面部5aが面接触する場合の方が、第2領域G2のスクライブ線Sの近傍に作用する曲げ応力が大きくなる。また、この過程では、板状部材5の平面部5aは、第2領域G2の表面Gxを滑動し、第2領域G2に対する相対位置が、スクライブ線Sから離反する側に移動する。これに対して、吸着パッド7の第2領域G2に対する相対位置は変化しない。 Next, as shown in FIG. 4B, the roller 10 and the roller shaft 9 are linearly moved (translated) in the direction D, so that the planar portion 5a of the plate-like member 5 is moved to the surface Gx of the second region G2. , and rotates around the roller shaft 9 (axis 9a). As a result, the plate glass G bends with the back support member 3 as a starting point. At this time, the angle of the planar portion 5a of the plate member 5 changes following the angle change of the surface Gx of the second region G2. In this process, the portion from the surface contact portion Gw of the plate-like member 5 with the planar portion 5a in the second region G2 to the scribe line S becomes nearly flat. The vicinity of S has a shape close to bending, that is, a shape curved with a large curvature. Here, the curved line W indicated by the dashed line in FIG. It is a drawing of the shape when it is bent. This curved line W is curved with a small curvature in the vicinity of the scribe line S of the second region G2. Therefore, the bending stress acting in the vicinity of the scribe line S of the second region G2 is greater when the planar portion 5a of the plate member 5 is in surface contact than when the roller 10 is in direct contact. Also, in this process, the planar portion 5a of the plate-like member 5 slides on the surface Gx of the second region G2, and the relative position to the second region G2 moves away from the scribe line S. On the other hand, the position of the suction pad 7 relative to the second region G2 does not change.

この後、ローラ10及びローラ軸9がさらにD方向に直進移動して、板状部材5の平面部5aが第2領域G2をさらに押し込み、スクライブ線Sの近傍に作用する曲げ応力が十分に大きくなった時点で、図4(c)に示すように、板ガラスGがスクライブ線Sに沿って割断される。この場合、図4(b)に基づいて既に説明したように、第2領域G2が撓んだ時には、第2領域G2の面接触部Gwからスクライブ線Sに至るまでの部位が平坦に近い形状になる。そのため、ローラ10をD方向に直進移動させる距離が短くても、板ガラスGを割断することができる。これにより、板ガラスGの割断に要する時間が短縮され、作業効率が向上すると共に、ローラ付き部材8を移動させる機構のコンパクト化も図られる。なお、板ガラスGが割断されることで第2領域G2が第1領域G1から分離した後は、第2領域G2は落下することなく、吸着パッド7によって吸着保持された状態を維持する。そして、この第2領域G2は、第1領域G1に影響が生じない退避位置まで搬送された後、吸着パッド7による吸着が解除されて落下回収される。 After that, the roller 10 and the roller shaft 9 further move straight in the direction D, the planar portion 5a of the plate member 5 pushes the second region G2 further, and the bending stress acting in the vicinity of the scribe line S becomes sufficiently large. At this point, the sheet glass G is cut along the scribe lines S as shown in FIG. 4(c). In this case, as already described with reference to FIG. 4B, when the second region G2 is bent, the portion from the surface contact portion Gw of the second region G2 to the scribe line S has a nearly flat shape. become. Therefore, even if the distance for moving the roller 10 straight in the D direction is short, the plate glass G can be cut. As a result, the time required for breaking the plate glass G can be shortened, the work efficiency can be improved, and the mechanism for moving the member 8 with rollers can be made compact. After the second region G2 is separated from the first region G1 by breaking the sheet glass G, the second region G2 does not drop and maintains a state of being sucked and held by the suction pad 7. FIG. After the second area G2 is transported to a retracted position where the first area G1 is not affected, the suction by the suction pad 7 is released and the second area G2 is dropped and collected.

本発明に係る板ガラスの製造装置及び製造方法は、上記例示の構成に代えて、図5(a)に示すように、板状部材5の平面部5aが、第2領域G2のスクライブ線Sと対向する端縁部Gzを含む部位の表面Gxに接触するようにしてもよい。詳述すると、第2領域G2の端縁部Gz(耳部と呼称される部位)は、第2領域G2のその他の部位よりも厚みが大きく且つ上下方向(同図の奥行方向)において凹凸が形成されている。そのため、特許文献1に開示のようにローラを第2領域G2の端縁部Gzまたはその近傍の表面Gxに接触させた場合には、ローラがD方向に直進移動していく過程でローラと端縁部Gzとの不安定な接触に起因して両者間にガタツキ等が生じるおそれがある。これに対して、板状部材5の平面部5aが当該端縁部Gzを含む部位に接触している場合には、板状部材5をD方向に直進移動させても、板状部材5の平面部5aと端縁部Gzとの接触状態が安定するため、両者間にガタツキ等が生じ難くなる。また、図5(a)に示す板ガラスGは、第2領域G2の幅方向の寸法が短くなっている。このような第2領域G2の幅狭に対しては、板状部材5の平面部5aを、当該端縁部Gzの表面に接触させること、図例では端縁部Gzから食み出させることで、対応が可能である。 In the plate glass manufacturing apparatus and manufacturing method according to the present invention, instead of the configuration illustrated above, as shown in FIG. It may be in contact with the surface Gx of the portion including the opposing edge portion Gz. More specifically, the edge portion Gz of the second region G2 (a portion called an ear portion) is thicker than the other portions of the second region G2 and has irregularities in the vertical direction (the depth direction in the figure). formed. Therefore, when the roller is brought into contact with the edge portion Gz of the second region G2 or the surface Gx in the vicinity thereof as disclosed in Patent Document 1, the roller and the edge portion contact the roller during the straight movement in the D direction. Unstable contact with the edge Gz may cause rattling or the like between the two. On the other hand, when the planar portion 5a of the plate-like member 5 is in contact with the portion including the edge portion Gz, even if the plate-like member 5 is linearly moved in the D direction, the plate-like member 5 Since the contact state between the plane portion 5a and the edge portion Gz is stabilized, rattling or the like is less likely to occur between them. Further, in the plate glass G shown in FIG. 5(a), the dimension in the width direction of the second region G2 is short. In order to make the width of the second region G2 narrow, the planar portion 5a of the plate member 5 is brought into contact with the surface of the edge portion Gz, and is protruded from the edge portion Gz in the illustrated example. and can be handled.

さらに、図5(b)に示すように、板状部材5が可撓性を有するようにすれば、第2領域G2の端縁部Gzからその近傍にかけて板状部材5の平面部5aを隙間なくまたは僅かに隙間が生じた状態で面接触させることができる。詳述すると、板状部材5の剛性が板ガラスGの剛性よりも高く且つ板状部材5が可撓性を有するものであれば、同図に示すように、板状部材5が第2領域G2を変形させた上で、板状部材5自体も変形する態様となる。 Furthermore, as shown in FIG. 5(b), if the plate-like member 5 is made flexible, the flat portion 5a of the plate-like member 5 can be formed into a gap from the edge portion Gz of the second region G2 to the vicinity thereof. Surface contact can be made without or with a slight gap. More specifically, if the rigidity of the plate-like member 5 is higher than that of the plate glass G and the plate-like member 5 has flexibility, then the plate-like member 5 will be in the second region G2 as shown in FIG. is deformed, the plate member 5 itself is also deformed.

また、本発明に係る板ガラスの製造装置及び製造方法は、以上の説明に係る板ガラスGよりも反りが小さいかまたは反りが無い板ガラスを割断する場合に、以下に示すように構成を変更することができる。すなわち、まず、ローラ付き部材8の結束バンド12を外して、板状部材5を取り外す。その後、図6に示すように、第2領域G2の表面Gxにローラ10を転動可能に接触させると共に、第2領域G2の裏面Gyを吸着パッド7により吸着保持させる。この状態を初期状態とする。そして、この初期状態から、ローラ10をD方向に直進移動させることで、既述の図4(b)に示す状態のように第2領域G2を撓ませる。この過程では、ローラ10は、第2領域G2との間に生じる摩擦によって第2領域G2の表面Gxを転動し、これに伴ってローラ10の第2領域G2に対する相対位置がスクライブ線Sから離反する方向に移動する。そして、第2領域G2の撓みが大きくなり、スクライブ線Sに作用する曲げ応力が十分な大きさになった時点で、既述の図4(c)に示す状態のように板ガラスGが割断される。 In addition, the plate glass manufacturing apparatus and manufacturing method according to the present invention can be modified as follows when cutting a plate glass having a smaller warp or no warp than the plate glass G according to the above description. can. That is, first, the banding band 12 of the member 8 with rollers is removed, and the plate member 5 is removed. Thereafter, as shown in FIG. 6, the roller 10 is brought into rolling contact with the front surface Gx of the second region G2, and the rear surface Gy of the second region G2 is held by the suction pad 7 by suction. Let this state be the initial state. Then, from this initial state, the roller 10 is moved straight in the direction D, so that the second region G2 is bent as in the state shown in FIG. 4B. In this process, the roller 10 rolls on the surface Gx of the second region G2 due to friction generated between the roller 10 and the second region G2. move away from it. Then, when the deflection of the second region G2 becomes large and the bending stress acting on the scribe line S becomes sufficiently large, the sheet glass G is cut as in the state shown in FIG. 4(c). be.

さらに、本発明に係る板ガラスの製造装置及び製造方法は、板ガラスGを一箇所で割断するだけでなく、以下に示すように板ガラスGを二箇所で割断する場合にも適用可能である。すなわち、図7に示すように、板ガラスGの幅方向の中央側領域を第1領域G1として、その両側にスクライブ線Sを形成し、各スクライブ線Sの幅方向の外側領域をそれぞれ第2領域G2とする。そして、各第2領域G2の表面Gx側に、ローラ付き部材8をそれぞれ配置し、各第2領域G2の裏面Gy側に、吸着機構4をそれぞれ配置する。また、第1領域G1の幅方向の両端部における裏面Gb側に、裏面支持部材3をそれぞれ配置する。この場合には、各ローラ付き部材8を基準にすれば、幅方向の中央側が図1の矢印A方向側になり且つ幅方向の両外側が図1の矢印B方向側になる。これらを前提条件にすれば、板ガラスGの幅方向の両側でそれぞれ、既に説明した作用と実質的に同一の作用が行われ、且つ、既に説明した効果と実質的に同一の効果が得られる。 Furthermore, the manufacturing apparatus and manufacturing method of sheet glass according to the present invention can be applied not only to the case of breaking the sheet glass G at one point, but also to the case of breaking the sheet glass G at two points as described below. That is, as shown in FIG. 7, the central region in the width direction of the sheet glass G is defined as a first region G1, the scribe lines S are formed on both sides thereof, and the outer regions in the width direction of each scribe line S are the second regions. Let it be G2. Then, the members with rollers 8 are arranged on the front surface Gx side of each second region G2, and the adsorption mechanisms 4 are arranged on the rear surface Gy side of each second region G2. In addition, the back surface support members 3 are arranged on the back surface Gb side at both ends in the width direction of the first region G1. In this case, if each member 8 with rollers is used as a reference, the center side in the width direction will be the direction of arrow A in FIG. 1, and both outer sides in the width direction will be the direction of arrow B in FIG. If these are preconditions, substantially the same action as the already explained action is performed on both sides of the sheet glass G in the width direction, and substantially the same effect as the already explained effect can be obtained.

また、本発明に係る板ガラスの製造装置及び製造方法は、板状部材5の平面部5aを回転可能に支持するために、以下に示すような構成を採用することができる。すなわち、図8に示すように、板状部材5の表側に固定したブラケット13に、板状部材5の平面部5aの回転中心となる軸14を挿通し、この軸14を、支持体15の裏側に固定したブラケット16により支持させる。これにより、板状部材5の平面部5aは、軸14(軸線14a)の廻りに回転可能となる。なお、支持体15は、ロボットアーム等の駆動手段の動作によって、初期状態にある第2領域G2の表面Gxと直交するD方向に移動する。これ以外にも、支持体15によって支持された軸の廻りに板状部材5の平面部5aが回転可能とされる他の機構を採用することができる。 In order to rotatably support the planar portion 5a of the plate-like member 5, the plate glass manufacturing apparatus and manufacturing method according to the present invention can employ the following configuration. That is, as shown in FIG. 8, a bracket 13 fixed to the front side of the plate-like member 5 is passed through a shaft 14 that serves as the center of rotation of the planar portion 5a of the plate-like member 5. It is supported by a bracket 16 fixed on the back side. As a result, the planar portion 5a of the plate-like member 5 is rotatable around the shaft 14 (axis line 14a). Note that the support 15 is moved in the D direction orthogonal to the surface Gx of the second region G2 in the initial state by the operation of the driving means such as the robot arm. In addition to this, another mechanism can be adopted in which the planar portion 5a of the plate-like member 5 is rotatable around the shaft supported by the support 15. FIG.

なお、以上の実施形態では、ローラ軸9(軸14)が、初期状態にある第2領域G2の表面Gxと直交するD方向に直進移動するように構成したが、これに代えて、D方向と角度をなす斜め方向に直進移動させてもよい。さらに、ローラ軸9(軸14)は、裏面支持部材3の近傍やスクライブ線Sの近傍を中心とする円軌道またはこれに類似する軌道などの湾曲軌道に沿って移動させてもよい。また、ローラ軸9(軸14)と保持基材6とを、同一の湾曲軌道(例えば上記の湾曲軌道)に沿って移動させてもよい。 In the above embodiment, the roller shaft 9 (shaft 14) is configured to move straight in the D direction orthogonal to the surface Gx of the second region G2 in the initial state. It may be moved straight in an oblique direction forming an angle with . Further, the roller shaft 9 (shaft 14) may be moved along a curved orbit such as a circular or similar orbit centered near the back support member 3 or near the scribe line S. Further, the roller shaft 9 (shaft 14) and the holding base material 6 may be moved along the same curved track (for example, the curved track described above).

また、以上の実施形態では、板ガラスGの反りが、板ガラスGの表面におけるスクライブ線S及びこれと平行な任意の仮想直線が湾曲する形状を呈したものであるが、これとは異なる形状を呈する反りであってもよい。 In the above embodiment, the warpage of the sheet glass G is such that the scribe line S on the surface of the sheet glass G and any imaginary straight line parallel to the scribe line S are curved. It may be warped.

さらに、以上の実施形態では、板ガラスGを縦姿勢で吊り下げ支持するようにしたが、板ガラスGを横姿勢(好ましくは水平姿勢)で平置きするものであってもよい。この場合は、板ガラスGの下面を裏面支持部材3で支持し、板ガラスGの第2領域G2の上面を板状部材5によって下面側(下方)に押し込むことになる。なお、板ガラスGの上面を裏面支持部材3で支持し、板ガラスGの第2領域G2の下面を板状部材5によって上面側(上方)に押し込むようにしてもよい。また、板ガラスGの姿勢は、鉛直面や水平面に対して傾斜した傾斜姿勢でもよい。 Furthermore, in the above embodiment, the sheet glass G is suspended and supported in a vertical position, but the sheet glass G may be placed horizontally in a lateral position (preferably in a horizontal position). In this case, the lower surface of the sheet glass G is supported by the back support member 3, and the upper surface of the second region G2 of the sheet glass G is pushed downward by the plate member 5. As shown in FIG. Alternatively, the upper surface of the sheet glass G may be supported by the back surface support member 3 and the lower surface of the second region G2 of the sheet glass G may be pushed toward the upper surface side (upward) by the plate member 5 . Further, the attitude of the plate glass G may be an inclined attitude inclined with respect to a vertical plane or a horizontal plane.

本発明に係る板ガラスの製造装置及び製造方法において、板状部材5の幅方向寸法L4(単位:mm、図2(a)参照)は、板ガラスGの第2領域G2の幅方向の寸法(mm)に対する百分率で、30%以上が好ましく、50%以上がより好ましく、70%以上が最も好ましい。これにより、第2領域のスクライブ線の近傍を大きな曲率で湾曲した形状にすることを促進できる。一方、板状部材5の幅方向の寸法L4の上限は、例えば90%とすることができる。板状部材5の長手方向寸法L5(単位:mm、図3(a)参照)は、板ガラスGの長手方向寸法(mm)に対する百分率で、例えば70%以上とすることができ、図3(a)のように100%以上であってもよい。板状部材5の厚みTは、例えば5~15mmとすることができる。 In the plate glass manufacturing apparatus and manufacturing method according to the present invention, the widthwise dimension L4 (unit: mm, see FIG. 2A) of the plate member 5 is the widthwise dimension of the second region G2 of the plate glass G (mm ), preferably 30% or more, more preferably 50% or more, and most preferably 70% or more. As a result, the vicinity of the scribe line of the second region can be promoted to have a curved shape with a large curvature. On the other hand, the upper limit of the dimension L4 in the width direction of the plate member 5 can be set to 90%, for example. The longitudinal dimension L5 (unit: mm, see FIG. 3(a)) of the plate member 5 is a percentage of the longitudinal dimension (mm) of the plate glass G, and can be, for example, 70% or more. ) may be 100% or more. The thickness T of the plate member 5 can be set to 5 to 15 mm, for example.

また、本発明に係る板ガラスの製造装置及び製造方法において、第2領域G2の表面Gxに接触する押し込み部材は、板状部材5に限定されない。例えば、押し込み部材は、断面が半円形、三角形、四角形、或いはその他の多角形からなる柱状体や、これら以外の立体形状をなすものであっても、平面部を有する部材であればよい。また、押し込み部材は、上下方向に長尺な単一の部材でなくてもよく、上下方向に沿って複数の押し込み部材が配列されるようにしてもよい。但し、この場合には、同一の軸線の廻りに同一の径で複数の押し込み部材が回転するように構成する必要がある。 In addition, in the plate glass manufacturing apparatus and manufacturing method according to the present invention, the pressing member that contacts the surface Gx of the second region G2 is not limited to the plate member 5 . For example, the pushing member may be a columnar body having a semicircular, triangular, quadrangular, or other polygonal cross-section, or a member having a three-dimensional shape other than these, as long as it has a flat portion. Also, the pushing member may not be a single member elongated in the vertical direction, and a plurality of pushing members may be arranged along the vertical direction. However, in this case, it is necessary to configure a plurality of pushing members to rotate around the same axis with the same diameter.

1 板ガラスの製造装置(割断装置)
3 裏面支持部材
5 板状部材(押し込み部材)
5a 平面部
7 吸着パッド
8 ローラ付き部材
9 ローラ軸
9a 軸線
10 ローラ
14 軸
14a 軸線
G 板ガラス
G1 第1領域
G2 第2領域
Ga 第1領域の表面
Gb 第1領域の裏面
Gx 第2領域の表面
Gy 第2領域の裏面
Gz 板ガラスの端縁部
S スクライブ線
1 Plate glass manufacturing equipment (cutting equipment)
3 back support member 5 plate-shaped member (push-in member)
5a Flat portion 7 Suction pad 8 Member with roller 9 Roller shaft 9a Axis 10 Roller 14 Axis 14a Axis G Plate glass G1 First region G2 Second region Ga Front surface Gb of first region Back surface Gx of first region Surface Gy of second region Rear surface Gz of second region Edge portion S of plate glass Scribe line

Claims (9)

板ガラスの第1領域と第2領域との境界部の表面側にスクライブ線を形成し、前記スクライブ線に沿って前記板ガラスを割断する割断工程を含む板ガラスの製造方法において、
前記割断工程では、裏面支持部材が前記第1領域の裏面を支持した状態にある時に、押し込み部材の平面部が前記第2領域の表面に接触した状態で回転しながら該第2領域を裏面側に押し込むことによって、前記スクライブ線に沿って前記板ガラスを割断することを特徴とする板ガラスの製造方法。
A method for producing a sheet glass, comprising a step of forming a scribe line on the surface side of a boundary between a first region and a second region of the sheet glass, and cutting the sheet glass along the scribe line,
In the cutting step, when the back surface supporting member is in a state of supporting the back surface of the first region, the flat portion of the pressing member is rotated while being in contact with the surface of the second region, and the second region is cut to the back side. A method for producing sheet glass, characterized in that the sheet glass is cut along the scribe line by pressing into.
前記平面部は、前記スクライブ線に沿う方向に延びる軸線の廻りに回転することを特徴とする請求項1に記載の板ガラスの製造方法。 2. The method of manufacturing sheet glass according to claim 1, wherein the planar portion rotates around an axis extending along the scribe line. 前記軸線は、前記平面部が前記第2領域を裏面側に押し込む方向に平行移動することを特徴とする請求項2に記載の板ガラスの製造方法。 3. The method of manufacturing sheet glass according to claim 2, wherein the axis moves in parallel in a direction in which the flat portion pushes the second region toward the back side. 前記平面部が前記第2領域を裏面側に押し込むことに伴う前記第2領域の前記平面部との接触部位の角度変化に追随して、前記平面部の角度が変化することを特徴とする請求項3に記載の板ガラスの製造方法。 The angle of the flat portion changes according to the angle change of the contact portion of the second region with the flat portion caused by the flat portion pushing the second region toward the rear surface side. Item 4. A method for producing plate glass according to item 3. 前記割断工程では、前記板ガラスを、前記スクライブ線が上下方向を向くように吊り下げ支持することを特徴とする請求項1~4の何れかに記載の板ガラスの製造方法。 5. The method for manufacturing a sheet glass according to claim 1, wherein in the cutting step, the sheet glass is suspended so that the scribe lines are oriented vertically. 前記割断工程では、前記第2領域の裏面を吸着保持することを特徴とする請求項1~5の何れかに記載の板ガラスの製造方法。 6. The method for producing sheet glass according to claim 1, wherein in the cutting step, the back surface of the second region is held by suction. 前記平面部は、前記第2領域の前記スクライブ線と対向する端縁部を含む部位の表面に接触することを特徴とする請求項1~6の何れかに記載の板ガラスの製造方法。 7. The method of manufacturing sheet glass according to claim 1, wherein the planar portion contacts the surface of the portion including the edge portion facing the scribe line of the second region. 前記押し込み部材は、板厚方向で対向する二つの表面のうちの一方の表面が前記平面部とされた板状部材であって、前記板状部材は、前記スクライブ線に沿う方向に延びる軸線の廻りに回転可能なローラを有するローラ付き部材に着脱可能に保持されていることを特徴とする請求項1~7の何れかに記載の板ガラスの製造方法。 The pressing member is a plate-like member having one of two surfaces facing each other in the plate thickness direction as the flat portion, and the plate-like member has an axis extending in a direction along the scribe line. 8. The method for producing sheet glass according to claim 1, wherein the plate glass is detachably held by a roller-equipped member having a roller rotatable therearound. 第1領域と第2領域との境界部の表面側にスクライブ線が形成された板ガラスを、前記スクライブ線に沿って割断する割断装置を備えた板ガラスの製造装置において、
前記割断装置は、前記第1領域の裏面を支持する裏面支持部材と、前記スクライブ線に沿って前記板ガラスを割断するために、前記第2領域の表面に接触した状態で回転しながら該第2領域を裏面側に押し込む平面部が形成された押し込み部材とを備えていることを特徴とする板ガラスの製造装置。
In a plate glass manufacturing apparatus equipped with a breaking device for breaking a plate glass having a scribe line formed on the surface side of a boundary portion between a first region and a second region along the scribe line,
The breaking device includes a back surface supporting member that supports the back surface of the first region, and a second cutting device that rotates while being in contact with the surface of the second region in order to cut the sheet glass along the scribe line. A sheet glass manufacturing apparatus, comprising: a pressing member having a flat portion for pressing a region toward the back side.
JP2019185419A 2019-10-08 2019-10-08 Sheet glass manufacturing method and its manufacturing apparatus Active JP7336071B2 (en)