JP6291702B2 - Thermoplastic resin composition and molded article thereof - Google Patents

Thermoplastic resin composition and molded article thereof Download PDF

Info

Publication number
JP6291702B2
JP6291702B2 JP2014084810A JP2014084810A JP6291702B2 JP 6291702 B2 JP6291702 B2 JP 6291702B2 JP 2014084810 A JP2014084810 A JP 2014084810A JP 2014084810 A JP2014084810 A JP 2014084810A JP 6291702 B2 JP6291702 B2 JP 6291702B2
Authority
JP
Japan
Prior art keywords
ethylene
copolymer
parts
olefin
polymer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2014084810A
Other languages
Japanese (ja)
Other versions
JP2015203102A (en
Inventor
吉孝 内藤
吉孝 内藤
崇 岩永
崇 岩永
長谷 信隆
信隆 長谷
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsubishi Chemical Corp
UMG ABS Ltd
Original Assignee
Mitsubishi Chemical Corp
UMG ABS Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Chemical Corp, UMG ABS Ltd filed Critical Mitsubishi Chemical Corp
Priority to JP2014084810A priority Critical patent/JP6291702B2/en
Publication of JP2015203102A publication Critical patent/JP2015203102A/en
Application granted granted Critical
Publication of JP6291702B2 publication Critical patent/JP6291702B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、熱可塑性樹脂組成物およびその成形品に関する。   The present invention relates to a thermoplastic resin composition and a molded article thereof.

成形品の耐衝撃性を向上させることによって、成形品の用途が拡大するだけでなく、成形品の薄肉化や大型化への対応が可能になるなど、工業的な有用性が非常に高くなる。そのため、成形品の耐衝撃性の向上については、これまでに様々な手法が提案されている。
これら手法のうち、ゴム質重合体と硬質樹脂とを組み合わせた樹脂材料を用いることによって、硬質樹脂に由来する特性を保持しつつ、成形品の耐衝撃性を高める手法は、すでに工業化されている。このような樹脂材料としては、アクリロニトリル−ブタジエン−スチレン(ABS)樹脂、アクリロニトリル−スチレン−アクリル酸エステル(ASA)樹脂、アクリロニトリル−エチレン・α−オレフィン−スチレン(AES)樹脂、またはこれらをさらに硬質樹脂に添加した熱可塑性樹脂組成物等が挙げられる。
Improving the impact resistance of the molded product not only expands the applications of the molded product, but also makes it extremely useful for industrial applications, such as enabling the molded product to be made thinner and larger. . Therefore, various techniques have been proposed so far for improving the impact resistance of the molded product.
Among these methods, by using a resin material in which a rubber polymer and a hard resin are combined, a method for improving the impact resistance of a molded product while maintaining the characteristics derived from the hard resin has already been industrialized. . Examples of such resin materials include acrylonitrile-butadiene-styrene (ABS) resin, acrylonitrile-styrene-acrylic acid ester (ASA) resin, acrylonitrile-ethylene / α-olefin-styrene (AES) resin, or a hard resin thereof. The thermoplastic resin composition etc. which were added to are mentioned.

硬質樹脂に由来する特性を保持しつつ、耐衝撃性が向上した成形品を得ることができる熱可塑性樹脂組成物としては、例えば、下記のものが知られている。
(1)硬質樹脂であるメタクリル酸エステル樹脂に、AES樹脂を添加した熱可塑性樹脂組成物(特許文献1)。
(2)硬質樹脂であるマレイミド系共重合体に、AES樹脂を添加した熱可塑性樹脂組成物(特許文献2)。
(3)硬質樹脂であるメタクリル酸エステル樹脂に、AES樹脂およびASA樹脂を添加した熱可塑性樹脂組成物(特許文献3)。
For example, the following are known as thermoplastic resin compositions capable of obtaining a molded article having improved impact resistance while maintaining the characteristics derived from the hard resin.
(1) A thermoplastic resin composition obtained by adding an AES resin to a methacrylic ester resin which is a hard resin (Patent Document 1).
(2) A thermoplastic resin composition in which an AES resin is added to a maleimide copolymer that is a hard resin (Patent Document 2).
(3) A thermoplastic resin composition obtained by adding an AES resin and an ASA resin to a methacrylic ester resin which is a hard resin (Patent Document 3).

しかし、(1)、(2)の熱可塑性樹脂組成物では、成形品の耐衝撃性を向上させるためにAES樹脂を多量に添加する必要があるため、得られる成形品においては、メタクリル酸エステル樹脂に由来する表面硬度(耐傷付き性)やマレイミド系共重合体に由来する耐熱性が著しく低下する。また、成形品の耐衝撃性を向上させるために比較的粒子径の大きいAES樹脂を添加する必要があるため、得られる成形品においては、硬質樹脂に由来する発色性が低下する。
(3)の熱可塑性樹脂組成物では、成形品の発色性の低下を抑えるためにAES樹脂およびASA樹脂を添加しているが、AES樹脂のみを添加したときに比べて成形品の耐衝撃性が劣る。
However, in the thermoplastic resin compositions of (1) and (2), it is necessary to add a large amount of AES resin in order to improve the impact resistance of the molded product. The surface hardness (scratch resistance) derived from the resin and the heat resistance derived from the maleimide copolymer are significantly reduced. In addition, since it is necessary to add an AES resin having a relatively large particle size in order to improve the impact resistance of the molded product, the color developability derived from the hard resin is reduced in the obtained molded product.
In the thermoplastic resin composition of (3), AES resin and ASA resin are added in order to suppress a decrease in color developability of the molded product, but the impact resistance of the molded product is higher than when only the AES resin is added. Is inferior.

特開2005−132970号公報JP 2005-132970 A 特開2004−352842号公報JP 2004-352842 A 特開2004−346187号公報JP 2004-346187 A

本発明は、流動性が良好であり、得られる成形品の耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性に優れる熱可塑性樹脂組成物、および耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性に優れる成形品を提供する。   The present invention is a thermoplastic resin composition having good flowability and excellent scratch resistance, impact resistance, cold shock resistance, color development, and lubricity of the obtained molded article, and scratch resistance, impact resistance, To provide molded products with excellent cold shock resistance, color development and lubricity.

本発明は、以下の態様を包含する。
[1]質量平均分子量(Mw)が17×10〜35×10であり、分子量分布(Mw/Mn)が1〜3であるエチレン・α−オレフィン共重合体(A)または該エチレン・α−オレフィン共重合体(A)を架橋処理した架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合して得られたグラフト共重合体(D)と、
ゴム状重合体(E)の存在下に、ビニル系単量体成分(m2)を重合して得られたグラフト共重合体(F)と、
メタクリル酸エステルを含むビニル系単量体成分(m3)を重合して得られたメタクリル酸エステル樹脂(G)と、
シリカ粒子(H)と、を含み、
前記グラフト重合体(D)に含まれるエチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の平均粒子径が、0.20μm〜0.60μmであり、
前記グラフト共重合体(F)に含まれるゴム状重合体(E)の平均粒子径が、0.05μm〜0.18μmであり、
前記エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)と前記ゴム状重合体(E)との合計(100質量%)のうち、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の割合が、15〜85質量%であり、ゴム状重合体(E)の割合が、85〜15質量%である、熱可塑性樹脂組成物。
[2]前記グラフト共重合体(D)が、前記架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合して得られたものである、[1]に記載の熱可塑性樹脂組成物。
[3][1]または[2]に記載の熱可塑性樹脂組成物を用いた成形品。
The present invention includes the following aspects.
[1] An ethylene / α-olefin copolymer (A) having a mass average molecular weight (Mw) of 17 × 10 4 to 35 × 10 4 and a molecular weight distribution (Mw / Mn) of 1 to 3, or the ethylene / Graft copolymer obtained by polymerizing vinyl monomer component (m1) in the presence of crosslinked ethylene / α-olefin copolymer (C) obtained by crosslinking α-olefin copolymer (A). (D),
A graft copolymer (F) obtained by polymerizing the vinyl monomer component (m2) in the presence of the rubber-like polymer (E);
A methacrylate ester resin (G) obtained by polymerizing a vinyl-based monomer component (m3) containing a methacrylate ester;
Silica particles (H),
The average particle diameter of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) contained in the graft polymer (D) is 0.20 μm to 0.60 μm,
The rubbery polymer (E) contained in the graft copolymer (F) has an average particle size of 0.05 μm to 0.18 μm,
Of the total (100% by mass) of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the rubbery polymer (E), ethylene / α-olefin The ratio of the copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) is 15 to 85% by mass, and the ratio of the rubbery polymer (E) is 85 to 15% by mass. Thermoplastic resin composition.
[2] The graft copolymer (D) is obtained by polymerizing the vinyl monomer component (m1) in the presence of the crosslinked ethylene / α-olefin copolymer (C). The thermoplastic resin composition according to [1].
[3] A molded article using the thermoplastic resin composition according to [1] or [2].

本発明の熱可塑性樹脂組成物は、流動性が良好である。また、本発明の熱可塑性樹脂組成物によれば、耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性に優れる成形品を得ることができる。
本発明の成形品は、耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性に優れる。
The thermoplastic resin composition of the present invention has good fluidity. In addition, according to the thermoplastic resin composition of the present invention, a molded product having excellent scratch resistance, impact resistance, cold impact resistance, color developability, and lubricity can be obtained.
The molded article of the present invention is excellent in scratch resistance, impact resistance, cold impact resistance, color development, and lubricity.

ガーゼ磨耗による耐擦り傷性試験を説明する概略図である。It is the schematic explaining the abrasion-resistance test by gauze wear. 潤滑性の評価方法を説明する概略図である。It is the schematic explaining the evaluation method of lubricity.

以下の用語の定義は、本明細書および特許請求の範囲にわたって適用される。
「(メタ)アクリル酸」とは、アクリル酸またはメタクリル酸を意味する。
「成形品」とは、熱可塑性樹脂組成物を成形してなるものを意味する。
「耐傷付き性」とは、爪等の硬く尖ったもので成形品の表面を引っ掻いたときに生じる傷(引っ掻き傷)に対する傷付きにくさ(耐引っ掻き傷性)および軍手、ガーゼ、布等の柔らかいもので成形品の表面を擦ったときに生じる傷(擦り傷)に対する傷付きにくさ(耐擦り傷性)の両方を意味する。
「明度(L)」とは、JIS Z 8729:2004において採用されているL表色系における色彩値のうちの明度の値(L)を意味する。
「SCE方式」とは、JIS Z 8722:2009に準拠した分光測色計を用い、光トラップによって正反射光を除去して色を測る方法を意味する。
The following definitions of terms apply throughout this specification and the claims.
“(Meth) acrylic acid” means acrylic acid or methacrylic acid.
“Molded product” means a product formed by molding a thermoplastic resin composition.
“Scratch resistance” refers to the resistance to scratches (scratch resistance) caused by scratching the surface of a molded article with a hard, pointed object such as a nail, and work gloves, gauze, cloth, etc. It means both scratch resistance (scratch resistance) against scratches (scratches) that occur when the surface of a molded product is rubbed with a soft material.
“Lightness (L * )” means the lightness value (L * ) of the color values in the L * a * b * color system adopted in JIS Z 8729: 2004.
The “SCE method” means a method of measuring a color by using a spectrocolorimeter compliant with JIS Z 8722: 2009 and removing specularly reflected light with an optical trap.

「熱可塑性樹脂組成物」
本発明の熱可塑性樹脂組成物は、グラフト共重合体(D)とグラフト共重合体(F)とメタクリル酸エステル樹脂(G)とシリカ粒子(H)とを含む。本発明の熱可塑性樹脂組成物は、本発明の効果を損なわない範囲内で、必要に応じて、スチレン系共重合体(I)、他の熱可塑性樹脂、各種添加剤を含んでいてもよい。
"Thermoplastic resin composition"
The thermoplastic resin composition of the present invention contains a graft copolymer (D), a graft copolymer (F), a methacrylic ester resin (G), and silica particles (H). The thermoplastic resin composition of the present invention may contain a styrenic copolymer (I), other thermoplastic resins, and various additives as necessary within the range not impairing the effects of the present invention. .

グラフト共重合体(D)は、下記(α)または(β)である。
(α)エチレン・α−オレフィン共重合体(A)の存在下に、ビニル系単量体成分(m1)を重合して得られたもの。
(β)架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合して得られたもの。
The graft copolymer (D) is the following (α) or (β).
(Α) A product obtained by polymerizing the vinyl monomer component (m1) in the presence of the ethylene / α-olefin copolymer (A).
(Β) A product obtained by polymerizing the vinyl monomer component (m1) in the presence of the crosslinked ethylene / α-olefin copolymer (C).

前記(α)として具体的には、エチレン・α−オレフィン共重合体(A)の水性分散体であるオレフィン樹脂水性分散体(B)中にてビニル系単量体成分(m1)を重合して得られたもの、エチレン・α−オレフィン共重合体(A)の溶液中にてビニル系単量体成分(m1)を重合して得られたもの等が挙げられる。   Specifically, the vinyl monomer component (m1) is polymerized in the olefin resin aqueous dispersion (B) which is an aqueous dispersion of the ethylene / α-olefin copolymer (A) as the (α). And those obtained by polymerizing the vinyl monomer component (m1) in a solution of the ethylene / α-olefin copolymer (A).

前記(β)として具体的には、架橋エチレン・α−オレフィン共重合体(C)の水性分散体中にてビニル系単量体成分(m1)を重合して得られたもの、架橋エチレン・α−オレフィン共重合体(C)の溶液中にてビニル系単量体成分(m1)を重合して得られたもの等が挙げられる。   Specifically, the (β) is obtained by polymerizing the vinyl monomer component (m1) in an aqueous dispersion of a crosslinked ethylene / α-olefin copolymer (C), Examples thereof include those obtained by polymerizing the vinyl monomer component (m1) in a solution of the α-olefin copolymer (C).

グラフト共重合体(F)は、ゴム状重合体(E)の存在下に、ビニル系単量体成分(m2)を重合して得られたものである。
メタクリル酸エステル樹脂(G)は、ビニル系単量体成分(m3)を重合して得られたものである。
スチレン系共重合体(I)は、ビニル系単量体成分(m4)を重合して得られたものである。
以下、各成分((A)〜(I)、(m1)〜(m4)等)について説明する。
The graft copolymer (F) is obtained by polymerizing the vinyl monomer component (m2) in the presence of the rubber-like polymer (E).
The methacrylic ester resin (G) is obtained by polymerizing the vinyl monomer component (m3).
The styrene copolymer (I) is obtained by polymerizing the vinyl monomer component (m4).
Hereinafter, each component ((A)-(I), (m1)-(m4) etc.) is demonstrated.

<エチレン・α−オレフィン共重合体(A)>
エチレン・α−オレフィン共重合体(A)は、エチレンと炭素数が3以上のα−オレフィンとを公知の重合方法によって共重合することによって得られた、エチレン単位とα−オレフィン単位とからなる共重合体である。
<Ethylene / α-olefin copolymer (A)>
The ethylene / α-olefin copolymer (A) comprises an ethylene unit and an α-olefin unit obtained by copolymerizing ethylene and an α-olefin having 3 or more carbon atoms by a known polymerization method. It is a copolymer.

α−オレフィンとしては、プロピレン、1−ブテン、1−ペンテン、1−ヘキセン、1−ヘプテン、1−オクテン、1−デセン、1−ウンデセン、1−イコセン、1−ドコセン等が挙げられ、成形品の耐衝撃性の点から、炭素数が3〜20のα−オレフィンが好ましく、プロピレンが特に好ましい。   Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-icosene, 1-docosene, etc. From the viewpoint of impact resistance, an α-olefin having 3 to 20 carbon atoms is preferable, and propylene is particularly preferable.

エチレン・α−オレフィン共重合体(A)のエチレン単位の含有率は、エチレン・α−オレフィン共重合体(A)を構成する全ての構成単位の合計を100質量%としたときに、45〜65質量%が好ましく、50〜60質量%がより好ましい。エチレン単位の含有率が前記範囲内であれば、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、潤滑性のバランスがさらに優れる。特に、エチレン単位の含有率が50〜60質量%であれば、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性がさらに向上する。   The ethylene unit content of the ethylene / α-olefin copolymer (A) is 45 to 45% when the total of all the structural units constituting the ethylene / α-olefin copolymer (A) is 100% by mass. 65 mass% is preferable and 50-60 mass% is more preferable. When the ethylene unit content is within the above range, the balance of the scratch resistance, impact resistance, cold impact resistance, and lubricity of the molded product is further improved. In particular, when the ethylene unit content is 50 to 60% by mass, the scratch resistance, impact resistance, and cold impact resistance of the molded product are further improved.

エチレン・α−オレフィン共重合体(A)の質量平均分子量(Mw)は、17×10〜35×10であり、26×10〜32×10が好ましい。質量平均分子量(Mw)が17×10よりも小さい場合には、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、潤滑性が劣る。一方、質量平均分子量(Mw)が35×10よりも大きい場合には、熱可塑性樹脂組成物の流動性および成形品の発色性が劣る。質量平均分子量(Mw)が26×10〜32×10であれば、熱可塑性樹脂組成物の流動性および成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性がさらに優れる。 The mass average molecular weight (Mw) of the ethylene / α-olefin copolymer (A) is 17 × 10 4 to 35 × 10 4 , and preferably 26 × 10 4 to 32 × 10 4 . When the mass average molecular weight (Mw) is smaller than 17 × 10 4 , the scratch resistance, impact resistance, cold impact resistance, and lubricity of the molded product are inferior. On the other hand, when the mass average molecular weight (Mw) is larger than 35 × 10 4 , the fluidity of the thermoplastic resin composition and the color developability of the molded product are inferior. When the mass average molecular weight (Mw) is 26 × 10 4 to 32 × 10 4 , the fluidity of the thermoplastic resin composition and the scratch resistance, impact resistance, and cold impact resistance of the molded product are further improved.

エチレン・α−オレフィン共重合体(A)の分子量分布(Mw/Mn)は、1〜3であり、1.9〜2.5が好ましい。分子量分布(Mw/Mn)が3よりも大きい場合には、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、潤滑性が劣る。分子量分布(Mw/Mn)が1.9〜2.5であれば、熱可塑性樹脂組成物の流動性および成形品の耐擦り傷性、耐衝撃性がさらに優れる。   The molecular weight distribution (Mw / Mn) of the ethylene / α-olefin copolymer (A) is 1 to 3, and preferably 1.9 to 2.5. When the molecular weight distribution (Mw / Mn) is larger than 3, the molded article has poor scratch resistance, impact resistance, cold impact resistance, and lubricity. When the molecular weight distribution (Mw / Mn) is 1.9 to 2.5, the fluidity of the thermoplastic resin composition, the scratch resistance and the impact resistance of the molded product are further improved.

エチレン・α−オレフィン共重合体(A)の質量平均分子量(Mw)および数平均分子量(Mn)は、ゲルパーミエーションクロマトグラフィ(GPC)を用いて測定し、標準ポリスチレンで換算した値である。   The mass average molecular weight (Mw) and the number average molecular weight (Mn) of the ethylene / α-olefin copolymer (A) are values measured by gel permeation chromatography (GPC) and converted to standard polystyrene.

エチレン・α−オレフィン共重合体(A)の結晶化度は、0%〜30%であることが好ましく、1%〜30%であることがさらに好ましい。結晶化度が前記範囲内であれば、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、潤滑性のバランスがさらに優れる。特に、結晶化度が1%〜30%であれば、耐擦り傷性、耐衝撃性、耐寒衝撃性、潤滑性がさらに向上する。エチレン・α−オレフィン共重合体(A)の結晶化度は、X線回折を測定し、結晶のピーク面積の割合から求められる。   The degree of crystallinity of the ethylene / α-olefin copolymer (A) is preferably 0% to 30%, more preferably 1% to 30%. When the crystallinity is within the above range, the balance of scratch resistance, impact resistance, cold shock resistance and lubricity of the molded product is further improved. In particular, when the crystallinity is 1% to 30%, the scratch resistance, impact resistance, cold impact resistance, and lubricity are further improved. The crystallinity of the ethylene / α-olefin copolymer (A) is determined from the ratio of the peak area of the crystal by measuring X-ray diffraction.

エチレン・α−オレフィン共重合体(A)の製造方法は、限定されない。エチレン・α−オレフィン共重合体(A)は、通常、メタロセン触媒またはチーグラー・ナッタ触媒を用いてエチレンとα−オレフィンとを重合することによって製造される。   The method for producing the ethylene / α-olefin copolymer (A) is not limited. The ethylene / α-olefin copolymer (A) is usually produced by polymerizing ethylene and an α-olefin using a metallocene catalyst or a Ziegler-Natta catalyst.

メタロセン触媒としては、遷移金属(ジルコニウム、チタン、ハフニウム等)にシクロペンタジエニル骨格を有する有機化合物、ハロゲン原子等が配位したメタロセン錯体と、有機アルミニウム化合物、有機ホウ素化合物等とを組み合わせた触媒が挙げられる。
チーグラー・ナッタ触媒としては、遷移金属(チタン、バナジウム、ジルコニウム、ハフニウム等)のハロゲン化物と有機アルミニウム化合物、有機ホウ素化合物等とを組み合わせた触媒が挙げられる。
As a metallocene catalyst, a catalyst obtained by combining an organic compound having a cyclopentadienyl skeleton with a transition metal (zirconium, titanium, hafnium, etc.), a metallocene complex in which a halogen atom or the like is coordinated, an organoaluminum compound, an organoboron compound, etc. Is mentioned.
Examples of the Ziegler-Natta catalyst include a catalyst in which a halide of a transition metal (titanium, vanadium, zirconium, hafnium, etc.) is combined with an organic aluminum compound, an organic boron compound, or the like.

重合方法としては、前記触媒の存在下に、エチレンとα−オレフィンとを溶媒中で共重合させる方法が挙げられる。溶媒としては、炭化水素溶媒(ベンゼン、トルエン、キシレン、ペンタン、ヘキサン、ヘプタン、オクタン等)が挙げられる。炭化水素溶媒は、1種を単独で用いてもよく、2種以上を混合して用いてもよい。また、原料のα−オレフィンを溶媒として用いてもよい。   Examples of the polymerization method include a method in which ethylene and an α-olefin are copolymerized in a solvent in the presence of the catalyst. Examples of the solvent include hydrocarbon solvents (benzene, toluene, xylene, pentane, hexane, heptane, octane, etc.). A hydrocarbon solvent may be used individually by 1 type, and 2 or more types may be mixed and used for it. Moreover, you may use the raw material alpha olefin as a solvent.

エチレン、α−オレフィンの供給量、水素等の分子量調節剤の種類や量、触媒の種類や量、反応温度、圧力等の反応条件を変更することによって、エチレン・α−オレフィン共重合体(A)のエチレン単位の含有率、質量平均分子量(Mw)および分子量分布(Mw/Mn)を調整することができる。   By changing the reaction conditions such as the supply amount of ethylene, α-olefin, the type and amount of molecular weight regulators such as hydrogen, the type and amount of catalyst, the reaction temperature, and the pressure, an ethylene / α-olefin copolymer (A ) Ethylene unit content, mass average molecular weight (Mw) and molecular weight distribution (Mw / Mn) can be adjusted.

<オレフィン樹脂水性分散体(B)>
オレフィン樹脂水性分散体(B)は、エチレン・α−オレフィン共重合体(A)を水性媒体に分散させたものである。
オレフィン樹脂水性分散体(B)は、その他の成分として、乳化剤、酸変性オレフィン重合体等を含有してもよい。
<Olefin resin aqueous dispersion (B)>
The aqueous olefin resin dispersion (B) is obtained by dispersing the ethylene / α-olefin copolymer (A) in an aqueous medium.
The aqueous olefin resin dispersion (B) may contain an emulsifier, an acid-modified olefin polymer, and the like as other components.

乳化剤としては、公知のものが挙げられ、例えば、長鎖アルキルカルボン酸塩、スルホコハク酸アルキルエステル塩、アルキルベンゼンスルホン酸塩等が挙げられる。
オレフィン樹脂水性分散体(B)中の乳化剤の含有量は、得られる熱可塑性樹脂組成物の熱着色を抑制でき、オレフィン樹脂水性分散体(B)の粒子径制御が容易である点から、エチレン・α−オレフィン共重合体(A)100質量部に対して1〜8質量部が好ましい。
Examples of the emulsifier include known ones, and examples thereof include long-chain alkyl carboxylates, sulfosuccinic acid alkyl ester salts, and alkylbenzene sulfonates.
Since the content of the emulsifier in the aqueous olefin resin dispersion (B) can suppress the thermal coloring of the resulting thermoplastic resin composition, the particle size of the aqueous olefin resin dispersion (B) can be easily controlled. -1-8 mass parts is preferable with respect to 100 mass parts of alpha-olefin copolymer (A).

酸変性オレフィン重合体としては、質量平均分子量が1,000〜5,000のオレフィン重合体(ポリエチレン、ポリプロピレン等)を、官能基を有する化合物(不飽和カルボン酸化合物等)で変性したものが挙げられる。不飽和カルボン酸化合物としては、例えば、アクリル酸、マレイン酸、イタコン酸、無水マレイン酸、無水イタコン酸、マレイン酸モノアミド等が挙げられる。
オレフィン樹脂水性分散体(B)中の酸変性オレフィン重合体の含有量は、エチレン・α−オレフィン共重合体(A)100質量部に対して、1〜40質量部が好ましい。酸変性オレフィン重合体の添加量が前記範囲内であれば、成形品の耐傷付き性と耐衝撃性のバランスがさらに優れる。
Examples of the acid-modified olefin polymer include those obtained by modifying an olefin polymer having a mass average molecular weight of 1,000 to 5,000 (polyethylene, polypropylene, etc.) with a compound having a functional group (such as an unsaturated carboxylic acid compound). It is done. Examples of the unsaturated carboxylic acid compound include acrylic acid, maleic acid, itaconic acid, maleic anhydride, itaconic anhydride, maleic acid monoamide, and the like.
The content of the acid-modified olefin polymer in the aqueous olefin resin dispersion (B) is preferably 1 to 40 parts by mass with respect to 100 parts by mass of the ethylene / α-olefin copolymer (A). When the addition amount of the acid-modified olefin polymer is within the above range, the balance between scratch resistance and impact resistance of the molded product is further improved.

オレフィン樹脂水性分散体(B)の調製方法は、限定されない。調製方法としては、例えば、公知の溶融混練手段(ニーダー、バンバリーミキサー、多軸スクリュー押出機等)でエチレン・α−オレフィン共重合体(A)および必要に応じて酸変性オレフィン重合体を溶融混練し、機械的せん断力を与えて分散させ、乳化剤を含む水性媒体に添加する方法;エチレン・α−オレフィン共重合体(A)および必要に応じて酸変性オレフィン重合体を炭化水素溶媒(ペンタン、ヘキサン、ヘプタン、ベンゼン、トルエン、キシレン等)に乳化剤とともに溶解し、水性媒体に添加して乳化させた後、十分に撹拌し、炭化水素溶媒を留去する方法等が挙げられる。   The preparation method of the olefin resin aqueous dispersion (B) is not limited. As a preparation method, for example, an ethylene / α-olefin copolymer (A) and, if necessary, an acid-modified olefin polymer are melt-kneaded by a known melt-kneading means (kneader, Banbury mixer, multi-screw extruder, etc.). And then adding to an aqueous medium containing an emulsifier; an ethylene / α-olefin copolymer (A) and optionally an acid-modified olefin polymer in a hydrocarbon solvent (pentane, Hexane, heptane, benzene, toluene, xylene, etc.) together with an emulsifier, added to an aqueous medium and emulsified, and then sufficiently stirred to distill off the hydrocarbon solvent.

オレフィン樹脂水性分散体(B)中のエチレン・α−オレフィン共重合体(A)の平均粒子径は、成形品の物性が優れる点から、0.20〜0.60μmであり、0.30〜0.50μmが好ましい。平均粒子径が前記範囲内であれば、成形品の耐衝撃性、耐寒衝撃性、発色性、耐擦り傷性、潤滑性に優れる。   The average particle diameter of the ethylene / α-olefin copolymer (A) in the olefin resin aqueous dispersion (B) is 0.20 to 0.60 μm from the viewpoint of excellent physical properties of the molded product, and is 0.30 to 0.30. 0.50 μm is preferable. When the average particle diameter is within the above range, the molded article is excellent in impact resistance, cold impact resistance, color development, scratch resistance and lubricity.

オレフィン樹脂水性分散体(B)中のエチレン・α−オレフィン共重合体(A)の平均粒子径を制御する方法としては、乳化剤の種類または使用量、酸変性オレフィン重合体の種類または含有量、混練時に加えるせん断力、温度条件等を調整する方法が挙げられる。   As a method for controlling the average particle size of the ethylene / α-olefin copolymer (A) in the olefin resin aqueous dispersion (B), the type or amount of the emulsifier, the type or content of the acid-modified olefin polymer, The method of adjusting the shear force, temperature conditions, etc. which are applied at the time of kneading | mixing is mentioned.

<架橋エチレン・α−オレフィン共重合体(C)>
架橋エチレン・α−オレフィン共重合体(C)は、エチレン・α−オレフィン共重合体(A)を架橋処理したものである。
エチレン・α−オレフィン共重合体(A)を架橋処理することにより、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、発色性、潤滑性のバランスがさらに優れる。
<Crosslinked ethylene / α-olefin copolymer (C)>
The crosslinked ethylene / α-olefin copolymer (C) is obtained by crosslinking the ethylene / α-olefin copolymer (A).
By crosslinking the ethylene / α-olefin copolymer (A), the balance of scratch resistance, impact resistance, cold impact resistance, color developability and lubricity of the molded product is further improved.

架橋エチレン・α−オレフィン共重合体(C)のゲル含有率は、成形品の耐擦り傷性、耐衝撃性、耐寒衝撃性、発色性、潤滑性とのバランスの点から、35〜75質量%が好ましく、40〜70質量%がより好ましく、45〜65質量%が特に好ましい。
ゲル含有率とは、架橋エチレン・α−オレフィン共重合体(C)をトルエンで膨潤させた場合の、膨潤前の架橋エチレン・α−オレフィン共重合体(C)に対する、乾燥させたトルエン不溶解分の割合である。
The gel content of the crosslinked ethylene / α-olefin copolymer (C) is 35 to 75% by mass from the viewpoint of the balance of scratch resistance, impact resistance, cold impact resistance, color development, and lubricity of the molded product. Is preferable, 40-70 mass% is more preferable, 45-65 mass% is especially preferable.
The gel content means that the crosslinked ethylene / α-olefin copolymer (C) is swollen with toluene and the dried toluene insoluble to the crosslinked ethylene / α-olefin copolymer (C) before swelling. The ratio of minutes.

エチレン・α−オレフィン共重合体(A)の架橋処理は、公知の方法によって行うことができる。架橋処理の方法としては、(a)エチレン・α−オレフィン共重合体(A)またはオレフィン樹脂水性分散体(B)に、有機過酸化物と、必要に応じて多官能性化合物とを添加して架橋処理を行う方法;(b)電離性放射線によって架橋処理を行う方法等が挙げられ、成形品の耐衝撃性、発色性の点から、(a)の方法が好ましい。   The crosslinking treatment of the ethylene / α-olefin copolymer (A) can be carried out by a known method. As a crosslinking treatment method, (a) an organic peroxide and, if necessary, a polyfunctional compound are added to the ethylene / α-olefin copolymer (A) or the aqueous olefin resin dispersion (B). (B) A method of performing a crosslinking treatment with ionizing radiation, and the like, and the method (a) is preferred from the viewpoint of impact resistance and color developability of the molded product.

(a)の方法としては、具体的には、エチレン・α−オレフィン共重合体(A)またはオレフィン樹脂水性分散体(B)に、有機過酸化物と、必要に応じて多官能性化合物とを添加し、加熱する方法等が挙げられる。
有機過酸化物および多官能性化合物の添加量、加熱温度、加熱時間等を調整することによって、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を調整できる。
加熱温度は、有機過酸化物の種類によって異なる。加熱温度は、有機過酸化物の10時間半減期温度の−5℃〜+30℃が好ましい。
加熱時間は、3〜15時間が好ましい。
Specifically, as the method of (a), an ethylene / α-olefin copolymer (A) or an aqueous olefin resin dispersion (B) is mixed with an organic peroxide and, if necessary, a multifunctional compound. The method of adding and heating is mentioned.
The gel content of the crosslinked ethylene / α-olefin copolymer (C) can be adjusted by adjusting the addition amount of organic peroxide and polyfunctional compound, heating temperature, heating time and the like.
The heating temperature varies depending on the type of organic peroxide. The heating temperature is preferably −5 ° C. to + 30 ° C., which is the 10-hour half-life temperature of the organic peroxide.
The heating time is preferably 3 to 15 hours.

有機過酸化物は、エチレン・α−オレフィン共重合体(A)に架橋構造を形成させるためのものである。有機過酸化物としては、例えば、ペルオキシエステル化合物、ペルオキシケタール化合物、ジアルキルペルオキシド化合物等が挙げられる。有機過酸化物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   The organic peroxide is for forming a crosslinked structure in the ethylene / α-olefin copolymer (A). Examples of the organic peroxide include a peroxy ester compound, a peroxy ketal compound, a dialkyl peroxide compound, and the like. An organic peroxide may be used individually by 1 type, and may be used in combination of 2 or more type.

ペルオキシエステル化合物の具体例としては、α,α’−ビス(ネオデカノイルペルオキシ)ジイソプロピルベンゼン、クミルペルオキシネオデカノエート、1,1,3,3−テトラメチルブチルペルオキシネオデカノエート、1−シクロヘキシル−1−メチルエチルペルオキシネオデカノエート、t−ヘキシルペルオキシネオデカノエート、t−ブチルペルオキシネオデカノエート、t−ヘキシルペルオキシピバレイト、t−ブチルペルオキシピバレート、1,1,3,3−テトラメチルブチルペルオキシ−2−エチルヘキサノエート、2,5−ジメチル−2,5−ビス(2−エチルヘキサノイルペルオキシ)ヘキサン、1−シクロヘキシル−1−メチルエチルペルオキシ−2−エチルヘキサノエート、t−ヘキシルペルオキシ2−ヘキシルヘキサノエート、t−ブチルペルオキシ2−ヘキシルヘキサノエート、t−ブチルペルオキシイソブチレート、t−ヘキシルペルオキシイソプロピルモノカーボネート、t−ブチルペルオキシマレイックアシッド、t−ブチルペルオキシ3,5,5−トリメチルヘキサノエート、t−ブチルペルオキシラウレート、2,5−ジメチル−2,5−ビス(m−トルオイルペルオキシ)ヘキサン、t−ブチルペルオキシイソプロピルモノカーボネート、t−ブチルペルオキシ2−エチルヘキシルモノカーボネート、t−ヘキシルペルオキシベンゾエート、2,5−ジメチル−2,5−ビス(ベンゾイルペルオキシ)ヘキサン、t−ブチルペルオキシアセテート、t−ブチルペルオキシ−m−トルオイルベンゾエート、t−ブチルペルオキシベンゾエート、ビス(t−ブチルペルオキシ)イソフタレート等が挙げられる。   Specific examples of the peroxyester compound include α, α′-bis (neodecanoylperoxy) diisopropylbenzene, cumylperoxyneodecanoate, 1,1,3,3-tetramethylbutylperoxyneodecanoate, 1 -Cyclohexyl-1-methylethylperoxyneodecanoate, t-hexylperoxyneodecanoate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, 1,1, 3,3-tetramethylbutylperoxy-2-ethylhexanoate, 2,5-dimethyl-2,5-bis (2-ethylhexanoylperoxy) hexane, 1-cyclohexyl-1-methylethylperoxy-2-ethyl Hexanoate, t-hexyl peroxy 2-hexyl Hexanoate, t-butylperoxy 2-hexylhexanoate, t-butylperoxyisobutyrate, t-hexylperoxyisopropyl monocarbonate, t-butylperoxymaleic acid, t-butylperoxy 3,5,5-trimethylhexano Ate, t-butylperoxylaurate, 2,5-dimethyl-2,5-bis (m-toluoylperoxy) hexane, t-butylperoxyisopropyl monocarbonate, t-butylperoxy 2-ethylhexyl monocarbonate, t-hexyl Peroxybenzoate, 2,5-dimethyl-2,5-bis (benzoylperoxy) hexane, t-butylperoxyacetate, t-butylperoxy-m-toluoylbenzoate, t-butylperoxybenzoe , Bis (t-butylperoxy) isophthalate.

ペルオキシケタール化合物の具体例としては、1,1−ビス(t−ヘキシルペルオキシ)3,3,5−トリメチルシクロヘキサン、1,1−ビス(t−ヘキシルペルオキシ)シクロヘキサン、1,1−ビス(t−ブチルペルオキシ)3,3,5−トリメチルシクロヘキサン、1,1−ビス(t−ブチルペルオキシ)シクロヘキサン、1,1−ビス(t−ブチルペルオキシ)シクロドデカン、2,2−ビス(t−ブチルペルオキシ)ブタン、n−ブチル4,4−ビス(t−ブチルペルオキシ)バレレート、2,2−ビス(4,4−ジ−t−ブチルペルオキシシクロヘキシル)プロパン等が挙げられる。   Specific examples of the peroxyketal compound include 1,1-bis (t-hexylperoxy) 3,3,5-trimethylcyclohexane, 1,1-bis (t-hexylperoxy) cyclohexane, 1,1-bis (t- Butylperoxy) 3,3,5-trimethylcyclohexane, 1,1-bis (t-butylperoxy) cyclohexane, 1,1-bis (t-butylperoxy) cyclododecane, 2,2-bis (t-butylperoxy) Examples include butane, n-butyl 4,4-bis (t-butylperoxy) valerate, 2,2-bis (4,4-di-t-butylperoxycyclohexyl) propane, and the like.

ジアルキルペルオキシド化合物の具体例としては、α,α’−ビス(t−ブチルペルオキシド)ジイソプロピルベンゼン、ジクミルペルオキシド、2,5−ジメチル−2,5−ビス(t−ブチルペルオキシ)ヘキサン、t−ブチルクミルペルオキシド、ジ−t−ブチルペルオキシド、2,5−ジメチル−2,5−ビス(t−ブチルペルオキシ)ヘキシン−3等が挙げられる。   Specific examples of the dialkyl peroxide compound include α, α′-bis (t-butyl peroxide) diisopropylbenzene, dicumyl peroxide, 2,5-dimethyl-2,5-bis (t-butylperoxy) hexane, and t-butyl. Examples include cumyl peroxide, di-t-butyl peroxide, 2,5-dimethyl-2,5-bis (t-butylperoxy) hexyne-3 and the like.

有機過酸化物としては、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を調整しやすい点から、ジクミルペルオキシド、t−ブチルクミルペルオキシド、ジ−t−ブチルペルオキシド等のジアルキルペルオキシド化合物が特に好ましい。   As the organic peroxide, dialkyl such as dicumyl peroxide, t-butylcumyl peroxide, di-t-butyl peroxide, etc., because it is easy to adjust the gel content of the crosslinked ethylene / α-olefin copolymer (C). Peroxide compounds are particularly preferred.

有機過酸化物の添加量は、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を35〜75質量%の範囲に調整しやすい点から、エチレン・α−オレフィン共重合体(A)100質量部に対して0.1〜5質量部が好ましい。   The addition amount of the organic peroxide is such that the gel content of the crosslinked ethylene / α-olefin copolymer (C) can be easily adjusted to a range of 35 to 75% by mass, so that the ethylene / α-olefin copolymer (A ) 0.1 to 5 parts by mass is preferable with respect to 100 parts by mass.

多官能性化合物は、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を調整するために、必要に応じて有機過酸化物と併用されるものである。
多官能性化合物としては、ジビニルベンゼン、メタクリル酸アリル、エチレングリコールジメタクリレート、1,3−ブチレンジメタクリレート、テトラエチレングリコールジアクリレート、トリアリルシアヌレート、トリアリルイソシアヌレート、ペンタエリスリトールテトラアクリレート等が挙げられ、ゲル含有率を調整しやすい点から、ジビニルベンゼンが好ましい。多官能性化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
The polyfunctional compound is used in combination with an organic peroxide as necessary in order to adjust the gel content of the crosslinked ethylene / α-olefin copolymer (C).
Examples of the multifunctional compound include divinylbenzene, allyl methacrylate, ethylene glycol dimethacrylate, 1,3-butylene dimethacrylate, tetraethylene glycol diacrylate, triallyl cyanurate, triallyl isocyanurate, pentaerythritol tetraacrylate, and the like. From the viewpoint of easily adjusting the gel content, divinylbenzene is preferable. A polyfunctional compound may be used individually by 1 type, and may be used in combination of 2 or more type.

多官能性化合物の添加量は、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を35〜75質量%に調整しやすい点から、エチレン・α−オレフィン共重合体(A)100質量部に対して10質量部以下が好ましい。   The addition amount of the polyfunctional compound is such that the gel content of the crosslinked ethylene / α-olefin copolymer (C) can be easily adjusted to 35 to 75% by mass, and thus the ethylene / α-olefin copolymer (A) 100 is used. 10 parts by mass or less is preferable with respect to parts by mass.

オレフィン樹脂水性分散体(B)に、有機過酸化物と、必要に応じて多官能性化合物とを添加して架橋処理すると、架橋エチレン・α−オレフィン共重合体(C)の水性分散体が得られる。該水性分散体は、その他の成分として、乳化剤、酸変性オレフィン重合体等を含有してもよい。乳化剤、酸変性オレフィン重合体はそれぞれ前記と同様のものが挙げられる。酸変性オレフィン重合体は、架橋処理されていてもよい。   When an organic peroxide and, if necessary, a polyfunctional compound are added to the olefin resin aqueous dispersion (B) and subjected to crosslinking treatment, an aqueous dispersion of the crosslinked ethylene / α-olefin copolymer (C) is obtained. can get. The aqueous dispersion may contain an emulsifier, an acid-modified olefin polymer and the like as other components. Examples of the emulsifier and the acid-modified olefin polymer are the same as those described above. The acid-modified olefin polymer may be subjected to a crosslinking treatment.

エチレン・α−オレフィン共重合体(A)に、有機過酸化物と、必要に応じて多官能性化合物とを添加し、溶融混練し、粉砕すると、架橋エチレン・α−オレフィン共重合体(C)の粉体が得られる。該粉体は、その他の成分として、酸変性オレフィン重合体等を含有してもよい。酸変性オレフィン重合体は前記と同様のものが挙げられる。酸変性オレフィン重合体は、架橋処理されていてもよい。   When an organic peroxide and, if necessary, a polyfunctional compound are added to the ethylene / α-olefin copolymer (A), melt-kneaded and pulverized, a crosslinked ethylene / α-olefin copolymer (C ) Powder is obtained. The powder may contain an acid-modified olefin polymer and the like as other components. Examples of the acid-modified olefin polymer are the same as described above. The acid-modified olefin polymer may be subjected to a crosslinking treatment.

酸変性オレフィン重合体の添加方法は、限定されない。エチレン・α−オレフィン共重合体(A)と酸変性オレフィン重合体とを混合した後に架橋処理をしてもよいし、エチレン・α−オレフィン共重合体(A)と酸変性オレフィン重合体とをそれぞれ架橋処理した後に混合してもよい。
エチレン・α−オレフィン共重合体(A)と酸変性オレフィン重合体との混合方法は、限定されない。混合方法としては、ニーダー、バンバリーミキサー、多軸スクリュー押出機等を用いた溶融混練法等が挙げられる。
The method for adding the acid-modified olefin polymer is not limited. Crosslinking may be performed after mixing the ethylene / α-olefin copolymer (A) and the acid-modified olefin polymer, or the ethylene / α-olefin copolymer (A) and the acid-modified olefin polymer. You may mix, after each crosslinking process.
The mixing method of the ethylene / α-olefin copolymer (A) and the acid-modified olefin polymer is not limited. Examples of the mixing method include a melt kneading method using a kneader, a Banbury mixer, a multi-screw extruder and the like.

架橋エチレン・α−オレフィン共重合体(C)の平均粒子径は、成形品の物性が優れる点から、0.20〜0.60μmであり、0.30〜0.50μmが好ましい。平均粒子径が前記範囲内であれば、成形品の耐衝撃性、耐寒衝撃性、発色性、耐擦り傷性、潤滑性に優れる。   The average particle size of the crosslinked ethylene / α-olefin copolymer (C) is 0.20 to 0.60 μm, preferably 0.30 to 0.50 μm, from the viewpoint of excellent physical properties of the molded product. When the average particle diameter is within the above range, the molded article is excellent in impact resistance, cold impact resistance, color development, scratch resistance and lubricity.

オレフィン樹脂水性分散体(B)に有機過酸化物等を添加し架橋処理して得られる水性分散体中の架橋エチレン・α−オレフィン共重合体(C)の平均粒子径は、オレフィン樹脂水性分散体(B)中のエチレン・α−オレフィン共重合体(A)の平均粒子径に対して変化はない。   The average particle size of the crosslinked ethylene / α-olefin copolymer (C) in the aqueous dispersion obtained by adding an organic peroxide or the like to the aqueous dispersion of the olefin resin (B) is olefin resin aqueous dispersion. There is no change with respect to the average particle diameter of the ethylene / α-olefin copolymer (A) in the body (B).

<ビニル系単量体成分(m1)>
ビニル系単量体成分(m1)は、芳香族ビニル化合物、シアン化ビニル化合物、他のビニル系単量体の群から選ばれる1種または2種以上の単量体からなる。
ビニル系単量体成分(m1)は、少なくとも芳香族ビニル化合物およびシアン化ビニル化合物を含むことが好ましい。
<Vinyl monomer component (m1)>
The vinyl monomer component (m1) is composed of one or more monomers selected from the group of aromatic vinyl compounds, vinyl cyanide compounds, and other vinyl monomers.
The vinyl monomer component (m1) preferably contains at least an aromatic vinyl compound and a vinyl cyanide compound.

芳香族ビニル化合物としては、例えば、スチレン、α−メチルスチレン、o−,m−またはp−メチルスチレン、ビニルキシレン、p−t−ブチルスチレン、エチルスチレン等が挙げられ、熱可塑性樹脂組成物の流動性、成形品の発色性、耐衝撃性の点から、スチレン、α−メチルスチレンが好ましい。芳香族ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the aromatic vinyl compound include styrene, α-methyl styrene, o-, m- or p-methyl styrene, vinyl xylene, pt-butyl styrene, ethyl styrene, and the like. Styrene and α-methylstyrene are preferable from the viewpoints of fluidity, color developability of molded products, and impact resistance. An aromatic vinyl compound may be used individually by 1 type, and may be used in combination of 2 or more type.

芳香族ビニル化合物の含有率は、ビニル系単量体成分(m1)100質量%中65〜82質量%が好ましく、73〜80質量%がより好ましく、75〜80質量%がさらに好ましい。芳香族ビニル化合物の含有率が前記範囲内であれば、成形品の発色性、耐衝撃性がさらに優れる。   65-82 mass% is preferable among 100 mass% of vinyl-type monomer components (m1), and, as for the content rate of an aromatic vinyl compound, 73-80 mass% is more preferable, and 75-80 mass% is further more preferable. When the content of the aromatic vinyl compound is within the above range, the color developability and impact resistance of the molded product are further improved.

シアン化ビニル化合物としては、例えば、アクリロニトリル、メタクリロニトリル等が挙げられる。シアン化ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the vinyl cyanide compound include acrylonitrile and methacrylonitrile. A vinyl cyanide compound may be used individually by 1 type, and may be used in combination of 2 or more type.

シアン化ビニル化合物の含有率は、ビニル系単量体成分(m1)100質量%中18〜35質量%が好ましく、20〜27質量%がより好ましく、20〜25質量%がさらに好ましい。シアン化ビニル化合物の含有率が前記範囲内であれば、成形品の発色性、耐衝撃性がさらに優れる。   The content of the vinyl cyanide compound is preferably 18 to 35% by mass, more preferably 20 to 27% by mass, and further preferably 20 to 25% by mass in 100% by mass of the vinyl monomer component (m1). When the content of the vinyl cyanide compound is within the above range, the color developability and impact resistance of the molded product are further improved.

他の単量体としては、アクリル酸エステル(アクリル酸メチル、アクリル酸エチル、アクリル酸プロピル、アクリル酸ブチル等)、メタクリル酸エステル(メタクリル酸メチル、メタクリル酸エチル、メタクリル酸プロピル、メタクリル酸ブチル等)、マレイミド系化合物(N−シクロヘキシルマレイミド、N−フェニルマレイミド等)等が挙げられる。他の単量体は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Other monomers include acrylic acid esters (methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, etc.), methacrylic acid esters (methyl methacrylate, ethyl methacrylate, propyl methacrylate, butyl methacrylate, etc.) ), Maleimide compounds (N-cyclohexylmaleimide, N-phenylmaleimide, etc.) and the like. Another monomer may be used individually by 1 type and may be used in combination of 2 or more type.

<グラフト共重合体(D)>
グラフト共重合体(D)は、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合することによって得られる。
<Graft copolymer (D)>
The graft copolymer (D) polymerizes the vinyl monomer component (m1) in the presence of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C). Can be obtained.

グラフト共重合体(D)は、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)50〜80質量%の存在下に、ビニル系単量体成分(m1)20〜50質量%(ただし、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とビニル系単量体成分(m1)との合計は100質量%である。)を重合して得られたものが好ましい。エチレン・α−オレフィン共重合体(A)が50〜80質量%であれば、熱可塑性樹脂組成物の流動性や、成形品の耐衝撃性、発色性の物性バランスがさらに向上する。   The graft copolymer (D) is a vinyl monomer component (in the presence of 50 to 80% by mass of an ethylene / α-olefin copolymer (A) or a crosslinked ethylene / α-olefin copolymer (C)). m1) 20-50% by mass (however, the total of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the vinyl monomer component (m1) is 100% by mass) %) Is preferred. When the ethylene / α-olefin copolymer (A) is 50 to 80% by mass, the fluidity of the thermoplastic resin composition, the impact resistance of the molded product, and the balance of physical properties of the coloring property are further improved.

グラフト共重合体(D)のグラフト率は、熱可塑性樹脂組成物の流動性および成形品の耐衝撃性、発色性のバランスの点から、20〜100質量%が好ましい。   The graft ratio of the graft copolymer (D) is preferably 20 to 100% by mass from the viewpoint of the balance between the fluidity of the thermoplastic resin composition, the impact resistance of the molded product, and the color development.

重合方法としては、公知の重合方法(乳化重合法、溶液重合法、懸濁重合法、塊状重合法等)が挙げられる。   Examples of the polymerization method include known polymerization methods (emulsion polymerization method, solution polymerization method, suspension polymerization method, bulk polymerization method, etc.).

乳化重合法によるグラフト共重合体(D)の製造方法としては、例えば、ビニル系単量体成分(m1)に有機過酸化物を混合した上で、ビニル系単量体成分(m1)をオレフィン樹脂水性分散体(B)または架橋エチレン・α−オレフィン共重合体(C)の水性分散液に連続的に添加する方法が挙げられる。
有機過酸化物は、有機過酸化物と遷移金属と還元剤とを組み合わせたレドックス系開始剤として用いるのが好ましい。
重合の際に、連鎖移動剤、乳化剤等を状況に応じて用いてもよい。
As a method for producing the graft copolymer (D) by emulsion polymerization, for example, an organic peroxide is mixed with the vinyl monomer component (m1), and then the vinyl monomer component (m1) is converted to olefin. Examples thereof include a method of continuously adding the aqueous resin dispersion (B) or the aqueous dispersion of the crosslinked ethylene / α-olefin copolymer (C).
The organic peroxide is preferably used as a redox initiator that combines an organic peroxide, a transition metal, and a reducing agent.
In the polymerization, a chain transfer agent, an emulsifier or the like may be used depending on the situation.

レドックス系開始剤としては、重合反応条件を高温下にする必要がなく、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の劣化等を避け、成形品の耐衝撃性の低下を回避できる点から、有機過酸化物と硫酸第一鉄−キレート剤−還元剤を組み合わせたものが好ましい。
有機過酸化物としては、クメンヒドロペルオキシド、ジイソプロピルベンゼンヒドロペルオキシド、t−ブチルヒドロペルオキシド等が挙げられる。
レドックス系開始剤としては、クメンヒドロペルオキシドと、硫酸第一鉄と、ピロリン酸ナトリウムと、デキストロースとからなるものがより好ましい。
The redox initiator does not require the polymerization reaction conditions to be at a high temperature, avoids deterioration of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C), and is molded. A combination of an organic peroxide and a ferrous sulfate-chelating agent-reducing agent is preferable from the viewpoint of avoiding a decrease in impact resistance of the product.
Examples of the organic peroxide include cumene hydroperoxide, diisopropylbenzene hydroperoxide, and t-butyl hydroperoxide.
The redox initiator is more preferably composed of cumene hydroperoxide, ferrous sulfate, sodium pyrophosphate, and dextrose.

連鎖移動剤としては、メルカプタン類(オクチルメルカプタン、n−またはt−ドデシルメルカプタン、n−ヘキサデシルメルカプタン、n−またはt−テトラデシルメルカプタン等)、アリル化合物(アリルスルフォン酸、メタアリルスルフォン酸、これらのナトリウム塩等)、α−メチルスチレンダイマー等が挙げられ、分子量を調整することが容易な点から、メルカプタン類が好ましい。連鎖移動剤は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
連鎖移動剤の添加方法は、一括、分割、連続のいずれでもよい。
連鎖移動剤の添加量は、ビニル単量体成分(m1)100質量部に対して2.0質量部以下が好ましい。
Examples of chain transfer agents include mercaptans (octyl mercaptan, n- or t-dodecyl mercaptan, n-hexadecyl mercaptan, n- or t-tetradecyl mercaptan, etc.), allyl compounds (allylsulfonic acid, methallylsulfonic acid, these Sodium salts, etc.), α-methylstyrene dimers, and the like, and mercaptans are preferred from the viewpoint of easy adjustment of the molecular weight. A chain transfer agent may be used individually by 1 type, and may be used in combination of 2 or more type.
The method for adding the chain transfer agent may be any of batch, split, and continuous.
The addition amount of the chain transfer agent is preferably 2.0 parts by mass or less with respect to 100 parts by mass of the vinyl monomer component (m1).

乳化剤としては、アニオン性界面活性剤、ノニオン性界面活性剤、両性界面活性剤等が挙げられる。
アニオン性界面活性剤としては、高級アルコールの硫酸エステル、アルキルベンゼンスルホン酸塩、脂肪酸スルホン酸塩、リン酸系塩、脂肪酸塩、アミノ酸誘導体塩等が挙げられる。
ノニオン性界面活性剤としては、通常のポリエチレングリコールのアルキルエステル型、アルキルエーテル型、アルキルフェニルエーテル型等が挙げられる。
両性界面活性剤としては、アニオン部にカルボン酸塩、硫酸エステル塩、スルホン酸塩、リン酸エステル塩等を有し、カチオン部にアミン塩、第4級アンモニウム塩等を有するものが挙げられる。
乳化剤の添加量は、ビニル単量体成分(m1)100質量部に対して10質量部以下が好ましい。
Examples of the emulsifier include anionic surfactants, nonionic surfactants, and amphoteric surfactants.
Examples of the anionic surfactants include higher alcohol sulfates, alkylbenzene sulfonates, fatty acid sulfonates, phosphate salts, fatty acid salts, and amino acid derivative salts.
Examples of nonionic surfactants include ordinary polyethylene glycol alkyl ester types, alkyl ether types, and alkyl phenyl ether types.
Examples of the amphoteric surfactant include those having a carboxylate salt, sulfate ester salt, sulfonate salt, phosphate ester salt and the like in the anion portion and amine salts and quaternary ammonium salts in the cation portion.
The amount of the emulsifier added is preferably 10 parts by mass or less with respect to 100 parts by mass of the vinyl monomer component (m1).

乳化重合法によって得られるグラフト共重合体(D)は、水中に分散した状態である。
グラフト共重合体(D)を含む水性分散体からグラフト共重合体(D)を回収する方法としては、例えば、水性分散体に析出剤を添加し、加熱、撹拌した後、析出剤を分離し、析出したグラフト共重合体(D)を水洗、脱水、乾燥する析出法が挙げられる。
析出剤としては、例えば、硫酸、酢酸、塩化カルシウム、硫酸マグネシウム等の水溶液が挙げられる。析出剤は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
グラフト共重合体(D)を含む水性分散体に、必要に応じて酸化防止剤を添加してもよい。
The graft copolymer (D) obtained by the emulsion polymerization method is in a state of being dispersed in water.
As a method for recovering the graft copolymer (D) from the aqueous dispersion containing the graft copolymer (D), for example, a precipitation agent is added to the aqueous dispersion, and after heating and stirring, the precipitation agent is separated. And a precipitation method in which the precipitated graft copolymer (D) is washed with water, dehydrated and dried.
Examples of the precipitating agent include aqueous solutions of sulfuric acid, acetic acid, calcium chloride, magnesium sulfate, and the like. A precipitation agent may be used individually by 1 type, and may be used in combination of 2 or more type.
An antioxidant may be added to the aqueous dispersion containing the graft copolymer (D) as necessary.

溶液重合法によるグラフト共重合体(D)の製造方法としては、例えば、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)を溶媒に溶解した溶液に、重合開始剤およびビニル系単量体成分(m1)を添加する方法が挙げられる。
溶媒としては、通常のラジカル重合で使用される不活性重合溶剤が用いられ、エチルベンゼン、トルエンなどの芳香族炭化水素、メチルエチルケトン、アセトンなどのケトン類、ジクロロメチレン、四塩化炭素などのハロゲン化炭化水素などが用いられる。
溶液重合に用いられる重合開始剤は、一般的な開始剤が用いられ、例えば、ケトンパーオキサイド、ジアルキルパーオキサイド、ジアシルパーオキサイド、パーオキシエステル、ハイドロパーオキサイドなどの有機過酸化物が用いられる。また、重合開始剤の添加方法としては、一括で添加する方法または連続的に添加する方法が挙げられる。
As a method for producing the graft copolymer (D) by the solution polymerization method, for example, an ethylene / α-olefin copolymer (A) or a crosslinked ethylene / α-olefin copolymer (C) is dissolved in a solvent. And a method of adding a polymerization initiator and a vinyl monomer component (m1).
As the solvent, an inert polymerization solvent used in ordinary radical polymerization is used, and aromatic hydrocarbons such as ethylbenzene and toluene, ketones such as methyl ethyl ketone and acetone, and halogenated hydrocarbons such as dichloromethylene and carbon tetrachloride. Etc. are used.
As the polymerization initiator used for the solution polymerization, a general initiator is used. For example, organic peroxides such as ketone peroxide, dialkyl peroxide, diacyl peroxide, peroxy ester, and hydroperoxide are used. Moreover, as the addition method of a polymerization initiator, the method of adding collectively and the method of adding continuously are mentioned.

<ゴム状重合体(E)>
ゴム状重合体(E)としては、特に制限はなく、ジエン系ゴム状重合体、アクリル系ゴム状重合体、オレフィン系ゴム状重合体、シリコーン系ゴム状重合体等が挙げられ、その他、ジエン系−アクリル系複合ゴム状重合体、シリコーン系−アクリル系複合ゴム状重合体等が挙げられる。
これらの中でも、耐候性に優れることからアクリル系ゴム状重合体、オレフィン系ゴム状重合体、シリコーン系ゴム状重合体、シリコーン系−アクリル系複合ゴム状重合が好ましく、耐衝撃性に優れることからシリコーン系−アクリル系複合ゴム状重合がより好ましい。これらは単独で用いてもよく、2種以上組み合わせて用いてもよい。
<Rubber polymer (E)>
The rubbery polymer (E) is not particularly limited, and examples thereof include diene rubbery polymers, acrylic rubbery polymers, olefinic rubbery polymers, silicone rubbery polymers, and the like. System-acrylic composite rubbery polymer, silicone-acrylic composite rubbery polymer, and the like.
Among these, acrylic rubber-like polymer, olefin rubber-like polymer, silicone rubber-like polymer, and silicone-acrylic composite rubber-like polymer are preferred because of excellent weather resistance, and because of excellent impact resistance. Silicone-acrylic composite rubbery polymerization is more preferred. These may be used alone or in combination of two or more.

ジエン系ゴム状重合体は、例えば、ブタジエン、イソプレン等のジエン成分と、必要に応じて、これらと共重合可能な単量体成分とを構成成分として含有するジエン系ゴム状重合体であり、ポリブタジエン、ポリイソプレン、スチレン−ブタジエン共重合体、アクリロニトリル−ブタジエン共重合体、ブタジエン−イソプレン−スチレン共重合体、ポリクロロプレン等が挙げられる。これらは1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   The diene rubber-like polymer is, for example, a diene rubber-like polymer containing a diene component such as butadiene and isoprene and, if necessary, a monomer component copolymerizable with these as constituent components. Examples include polybutadiene, polyisoprene, styrene-butadiene copolymer, acrylonitrile-butadiene copolymer, butadiene-isoprene-styrene copolymer, polychloroprene, and the like. These may be used individually by 1 type and may be used in combination of 2 or more type.

ジエン系ゴム状重合体の製造方法は特に限定されないが、公知の乳化重合法が好ましい。その際、乳化剤や重合開始剤、連鎖移動剤等も公知のものが利用できる。また粒子径の制御において、予め小粒子径のジエン系ゴム状重合体を製造し、さらにこれを公知の肥大化処理により粒子径を大きくしてもよい。   Although the manufacturing method of a diene rubber-like polymer is not specifically limited, The well-known emulsion polymerization method is preferable. At that time, known emulsifiers, polymerization initiators, chain transfer agents and the like can be used. In controlling the particle diameter, a diene rubbery polymer having a small particle diameter may be produced in advance, and the particle diameter may be increased by a known enlargement treatment.

アクリル系ゴム状重合体は、(メタ)アクリル酸エステルに由来する単位と、架橋剤に由来する単位およびグラフト交叉剤に由来する単位のいずれか一方または両方を有する共重合体であることが好ましい。
(メタ)アクリル酸エステルとしては、アルキル基の炭素数が1〜12である(メタ)アクリル酸アルキルエステル、芳香族炭化水素基(フェニル基、ベンジル基等)を有するアクリル酸エステル等が挙げられ、成形品の耐衝撃性の点から、アクリル酸n−ブチル、アクリル酸2−エチルヘキシル、アクリル酸エチルが好ましい。(メタ)アクリル酸エステルは、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
架橋剤としては、ジメタクリレート系化合物、具体例には、エチレングリコールジメタクリレート、プロピレングリコールジメタクリレート、1,3−ブチレングリコールジメタクリレート、1,4−ブチレングリコールジメタクリレート等が挙げられる。
グラフト交叉剤としては、アリル化合物、具体的には、メタクリル酸アリル、シアヌル酸トリアリル、イソシアヌル酸トリアリル等が挙げられる。
The acrylic rubber-like polymer is preferably a copolymer having one or both of a unit derived from a (meth) acrylic acid ester, a unit derived from a crosslinking agent, and a unit derived from a graft crossing agent. .
Examples of (meth) acrylic acid esters include (meth) acrylic acid alkyl esters having 1 to 12 carbon atoms in the alkyl group, and acrylic acid esters having an aromatic hydrocarbon group (such as a phenyl group or a benzyl group). From the viewpoint of impact resistance of the molded product, n-butyl acrylate, 2-ethylhexyl acrylate, and ethyl acrylate are preferable. One (meth) acrylic acid ester may be used alone, or two or more may be used in combination.
Examples of the crosslinking agent include dimethacrylate compounds, and specific examples include ethylene glycol dimethacrylate, propylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, and the like.
Examples of the grafting agent include allyl compounds, specifically, allyl methacrylate, triallyl cyanurate, triallyl isocyanurate, and the like.

アクリル系ゴム状重合体の製造方法は、特に制限されない。例えば、(メタ)アクリル酸エステルと、架橋剤およびグラフト交叉剤のいずれか一方または両方とを含む単量体成分を乳化重合してアクリル系ゴム状重合体の水性分散体を得る方法等が挙げられる。   The method for producing the acrylic rubbery polymer is not particularly limited. For example, a method of obtaining an aqueous dispersion of an acrylic rubber-like polymer by emulsion polymerization of a monomer component containing (meth) acrylic acid ester and one or both of a crosslinking agent and a graft crossing agent, etc. It is done.

オレフィン系ゴム状重合体は、例えば、エチレン・α−オレフィン共重合体、エチレン−プロピレン−非共役ジエン共重合体等が挙げられる。
エチレン・α−オレフィン共重合体のα−オレフィンとしては、炭素数が3以上のプロピレン、1−ブテン、1−ペンテン、1−ヘキセン、1−ヘプテン、1−オクテン、1−デセン、1−ウンデセン、1−イコセン、1−ドコセン等が挙げられる。α−オレフィンは1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
エチレン−プロピレン−非共役ジエン共重合体は、エチレン単位と、プロピレン単位と、第3成分である非共役ジエン単位とからなる共重合体である。
エチレン−プロピレン−非共役ジエン共重合体の非共役ジエンとしては、例えば、ジシクロペンタジエン、エチリデンノルボルネン、1,4−ヘキサジエン、1,5−ヘキサジエン、2−メチル−1,5−ヘキサジエン、1,4−シクロヘプタジエン、1,5−シクロオクタジエン等が挙げられる。非共役ジエンは1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
Examples of the olefin rubber-like polymer include an ethylene / α-olefin copolymer and an ethylene-propylene-nonconjugated diene copolymer.
Examples of the α-olefin of the ethylene / α-olefin copolymer include propylene having 3 or more carbon atoms, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene. 1-icosene, 1-docosene and the like. One α-olefin may be used alone, or two or more α-olefins may be used in combination.
The ethylene-propylene-nonconjugated diene copolymer is a copolymer comprising an ethylene unit, a propylene unit, and a nonconjugated diene unit that is a third component.
Examples of the non-conjugated diene of the ethylene-propylene-non-conjugated diene copolymer include dicyclopentadiene, ethylidene norbornene, 1,4-hexadiene, 1,5-hexadiene, 2-methyl-1,5-hexadiene, 1, Examples include 4-cycloheptadiene and 1,5-cyclooctadiene. A nonconjugated diene may be used individually by 1 type, and may be used in combination of 2 or more type.

オレフィン系ゴム状重合体の製造方法は、限定されない。例えば、オレフィン系ゴム状重合体は、通常、メタロセン触媒またはチーグラー・ナッタ触媒を用いてエチレンとα−オレフィンとを重合することによって製造される。
重合方法としては、触媒の存在下に、エチレンとα−オレフィンとを溶媒中で共重合させる方法が挙げられる。溶媒としては、炭化水素溶媒(ベンゼン、トルエン、キシレン、ペンタン、ヘキサン、ヘプタン、オクタン等)が挙げられる。炭化水素溶媒は、1種を単独で用いてもよく、2種以上を混合して用いてもよい。また、原料のα−オレフィンを溶媒として用いてもよい。
The method for producing the olefin rubber-like polymer is not limited. For example, an olefin rubber-like polymer is usually produced by polymerizing ethylene and an α-olefin using a metallocene catalyst or a Ziegler-Natta catalyst.
Examples of the polymerization method include a method of copolymerizing ethylene and α-olefin in a solvent in the presence of a catalyst. Examples of the solvent include hydrocarbon solvents (benzene, toluene, xylene, pentane, hexane, heptane, octane, etc.). A hydrocarbon solvent may be used individually by 1 type, and 2 or more types may be mixed and used for it. Moreover, you may use the raw material alpha olefin as a solvent.

オレフィン系ゴム状重合体は架橋処理されていてもよい。
架橋処理は、公知の方法によって行うことができる。架橋処理の方法としては、架橋エチレン・α−オレフィン共重合体(C)を得るときと同様の方法を用いることができる。
The olefin rubber-like polymer may be subjected to a crosslinking treatment.
The crosslinking treatment can be performed by a known method. As a method for the crosslinking treatment, the same method as that for obtaining the crosslinked ethylene / α-olefin copolymer (C) can be used.

オレフィン系ゴム状重合体は水性分散体であってもよい。
オレフィン系ゴム状重合体の水性分散体は、その他の成分として乳化剤、酸変性オレフィン重合体等を含有してもよい。
The olefin rubber-like polymer may be an aqueous dispersion.
The aqueous dispersion of the olefin rubber-like polymer may contain an emulsifier, an acid-modified olefin polymer and the like as other components.

乳化剤としては、公知のものが挙げられ、例えば、長鎖アルキルカルボン酸塩、スルホコハク酸アルキルエステル塩、アルキルベンゼンスルホン酸塩等が挙げられる。
酸変性オレフィン重合体としては、質量平均分子量が1,000〜5,000のオレフィン重合体(ポリエチレン、ポリプロピレン等)を、官能基を有する化合物(不飽和カルボン酸化合物等)で変性したものが挙げられる。不飽和カルボン酸化合物としては、例えば、アクリル酸、マレイン酸、イタコン酸、無水マレイン酸、無水イタコン酸、マレイン酸モノアミド等が挙げられる。
Examples of the emulsifier include known ones, and examples thereof include long-chain alkyl carboxylates, sulfosuccinic acid alkyl ester salts, and alkylbenzene sulfonates.
Examples of the acid-modified olefin polymer include those obtained by modifying an olefin polymer having a mass average molecular weight of 1,000 to 5,000 (polyethylene, polypropylene, etc.) with a compound having a functional group (such as an unsaturated carboxylic acid compound). It is done. Examples of the unsaturated carboxylic acid compound include acrylic acid, maleic acid, itaconic acid, maleic anhydride, itaconic anhydride, maleic acid monoamide, and the like.

オレフィン系ゴム状重合体の水性分散体の調製方法は、限定されない。調製方法としては、例えば、公知の溶融混練手段(ニーダー、バンバリーミキサー、多軸スクリュー押出機等)でオレフィン系ゴム状重合体および必要に応じて酸変性オレフィン重合体を溶融混練し、機械的せん断力を与えて分散させ、乳化剤を含む水性媒体に添加する方法;オレフィン系ゴム状重合体および必要に応じて酸変性オレフィン重合体を炭化水素溶媒(ペンタン、ヘキサン、ヘプタン、ベンゼン、トルエン、キシレン等)に乳化剤とともに溶解し、水性媒体に添加して乳化させた後、十分に撹拌し、炭化水素溶媒を留去する方法等が挙げられる。   The method for preparing the aqueous dispersion of the olefin rubber-like polymer is not limited. As a preparation method, for example, an olefin rubber-like polymer and, if necessary, an acid-modified olefin polymer are melt-kneaded by a known melt-kneading means (kneader, Banbury mixer, multi-screw extruder, etc.), and mechanical shearing is performed. A method of dispersing by applying force and adding to an aqueous medium containing an emulsifier; an olefin rubber-like polymer and, if necessary, an acid-modified olefin polymer in a hydrocarbon solvent (pentane, hexane, heptane, benzene, toluene, xylene, etc.) ) And an emulsifier, added to an aqueous medium and emulsified, and then sufficiently stirred to distill off the hydrocarbon solvent.

オレフィン系ゴム状重合体が架橋処理される場合、酸変性オレフィン重合体の添加方法は、限定されない。オレフィン系ゴム状重合体と酸変性オレフィン重合体とを混合した後に架橋処理をしてもよいし、オレフィン系ゴム状重合体と酸変性オレフィン重合体とをそれぞれ架橋処理した後に混合してもよい。   When the olefin rubber-like polymer is subjected to a crosslinking treatment, the method for adding the acid-modified olefin polymer is not limited. The olefin rubber-like polymer and the acid-modified olefin polymer may be mixed and then crosslinked, or the olefin rubber-like polymer and the acid-modified olefin polymer may be crosslinked and then mixed. .

シリコーン系ゴム状重合体は、ポリオルガノシロキサンであることが好ましい。
ポリオルガノシロキサンとしては、特に制限はないが、ビニル重合性官能基を有するポリオルガノシロキサンが好ましく、ビニル重合性官能基を含有するシロキサン単位0.3〜3モル%と、ジメチルシロキサン単位97〜99.7モル%とからなり、3個以上のシロキサン結合を有するケイ素原子がポリジメチルシロキサ中の全ケイ素原子に対し1モル%以下であるポリオルガノシロキサンがより好ましい。
ポリオルガノシロキサンには、必要に応じて、構成成分としてシロキサン系架橋剤が含まれていてもよい。
The silicone rubbery polymer is preferably a polyorganosiloxane.
Although there is no restriction | limiting in particular as polyorganosiloxane, The polyorganosiloxane which has a vinyl polymerizable functional group is preferable, 0.3-3 mol% of siloxane units containing a vinyl polymerizable functional group, and dimethylsiloxane units 97-99 are included. More preferred is a polyorganosiloxane composed of 0.7 mol% and having 3 or more siloxane bonds in silicon atoms of 1 mol% or less with respect to all silicon atoms in polydimethylsiloxa.
The polyorganosiloxane may contain a siloxane-based crosslinking agent as a constituent component, if necessary.

ジメチルシロキサンとしては、例えば、3員環以上のジメチルシロキサン系環状体が挙げられるが、中でも、3員環〜7員環のものが好ましい。具体的にはヘキサメチルシクロトリシロキサン、オクタメチルシクロテトラシロキサン、デカメチルシクロペンタシロキサン、ドデカメチルシクロヘキサシロキサン等が挙げられ、これらは1種でまたは2種以上を組み合わせて使用できる。   Examples of dimethylsiloxane include dimethylsiloxane-based cyclic bodies having three or more member rings, and among them, those having three to seven member rings are preferable. Specific examples include hexamethylcyclotrisiloxane, octamethylcyclotetrasiloxane, decamethylcyclopentasiloxane, dodecamethylcyclohexasiloxane, and the like. These can be used alone or in combination of two or more.

ビニル重合性官能基含有シロキサンとしては、ビニル重合性官能基を含有し、かつ、ジメチルシロキサンとシロキサン結合を介して結合しうるものであれば制限されないが、ジメチルシロキサンとの反応性を考慮すると、ビニル重合性官能基を含有する各種アルコキシシラン化合物が好ましい。具体的には、β−メタクリロイルオキシエチルジメトキシメチルシラン、γ−メタクリロイルオキシプロピルジメトキシメチルシラン、γ−メタクリロイルオキシプロピルメトキシジメチルシラン、γ−メタクリロイルオキシプロピルトリメトキシシラン、γ−メタクリロイルオキシプロピルエトキシジエチルシラン、γ−メタクリロイルオキシプロピルジエトキシメチルシランおよび∂−メタクリロイルオキシブチルジエトキシメチルシラン等のメタクリロイルオキシシロキサン、テトラメチルテトラビニルシクロテトラシロキサン等のビニルシロキサン、p−ビニルフエニルジメトキシメチルシランさらにγ−メルカプトプロピルジメトキシメチルシラン、γ−メルカプトプロピルトリメトキシシラン等のメルカプトシロキサンが挙げられる。これらビニル重合性官能基含有シロキサンは、1種でまたは2種以上を組み合わせて使用できる。   The vinyl polymerizable functional group-containing siloxane is not limited as long as it contains a vinyl polymerizable functional group and can be bonded to dimethylsiloxane via a siloxane bond, but considering the reactivity with dimethylsiloxane, Various alkoxysilane compounds containing a vinyl polymerizable functional group are preferred. Specifically, β-methacryloyloxyethyldimethoxymethylsilane, γ-methacryloyloxypropyldimethoxymethylsilane, γ-methacryloyloxypropylmethoxydimethylsilane, γ-methacryloyloxypropyltrimethoxysilane, γ-methacryloyloxypropylethoxydiethylsilane, methacryloyloxysiloxanes such as γ-methacryloyloxypropyldiethoxymethylsilane and ∂-methacryloyloxybutyldiethoxymethylsilane, vinylsiloxanes such as tetramethyltetravinylcyclotetrasiloxane, p-vinylphenyldimethoxymethylsilane and γ-mercaptopropyl Examples include mercaptosiloxanes such as dimethoxymethylsilane and γ-mercaptopropyltrimethoxysilane. These vinyl polymerizable functional group-containing siloxanes can be used alone or in combination of two or more.

シロキサン系架橋剤としては、3官能性または4官能性のシラン系架橋剤、例えばトリメトキシメチルシラン、トリエトキシフェニルシラン、テトラメトキシシラン、テトラエトキシシラン、テトラブトキシシラン等が挙げられる。   Examples of the siloxane crosslinking agent include trifunctional or tetrafunctional silane crosslinking agents such as trimethoxymethylsilane, triethoxyphenylsilane, tetramethoxysilane, tetraethoxysilane, and tetrabutoxysilane.

ポリオルガノシロキサンの製造方法は、限定されない。例えば、以下の方法により製造できる。
まず、ジメチルシロキサンとビニル重合性官能基を有するシロキサンとからなるシロキサン混合物に、必要に応じてシロキサン系架橋剤を添加し、次いで、乳化剤および水によって乳化させてシロキサン混合物水性分散体を得る。次いで、高速回転による剪断力で微粒子化するホモミキサーや、高圧発生機による噴出力で微粒子化するホモジナイザー等を使用して、シロキサン混合物水性分散体を微粒子化させる。ここで、ホモジナイザー等の高圧乳化装置を使用すると、ポリオルガノシロキサンの粒子径の分布が小さくなるので好ましい。次いで、微粒子化したシロキサン混合物水性分散体を、酸触媒を含む酸水溶液中に添加して高温下で重合させる。そして、反応液を冷却し、さらに苛性ソーダ、苛性カリ、炭酸ナトリウム等のアルカリ性物質で中和することで重合を停止させて、水性分散体に分散したポリオルガノシロキサンを得る。
The manufacturing method of polyorganosiloxane is not limited. For example, it can be produced by the following method.
First, a siloxane-based crosslinking agent is added to a siloxane mixture composed of dimethylsiloxane and a siloxane having a vinyl polymerizable functional group, if necessary, and then emulsified with an emulsifier and water to obtain an aqueous siloxane mixture dispersion. Next, the aqueous dispersion of the siloxane mixture is atomized using a homomixer that atomizes by a shearing force by high-speed rotation, a homogenizer that atomizes by a jet output from a high-pressure generator, or the like. Here, it is preferable to use a high-pressure emulsifier such as a homogenizer because the particle size distribution of the polyorganosiloxane becomes small. Next, the finely divided siloxane mixture aqueous dispersion is added to an acid aqueous solution containing an acid catalyst and polymerized at a high temperature. Then, the reaction solution is cooled and further neutralized with an alkaline substance such as caustic soda, caustic potash, sodium carbonate, or the like, to terminate the polymerization, and obtain a polyorganosiloxane dispersed in an aqueous dispersion.

上記ポリオルガノシロキサンの製造において、乳化剤としては、アニオン系乳化剤が好ましい。アニオン系乳化剤としては、例えば、アルキルベンゼンスルホン酸ナトリウム、ポリオキシエチレンノニルフェニルエーテル硫酸エステルナトリウムなどが挙げられる。これらの中でも、特にアルキルベンゼンスルホン酸ナトリウム、ラウリルスルホン酸ナトリウムなどのスルホン酸系の乳化剤が好ましい。これらの乳化剤は、シロキサン混合物100質量部(固形分として)に対して、0.05質量部〜 5質量部程度の範囲で使用される。   In the production of the polyorganosiloxane, the emulsifier is preferably an anionic emulsifier. Examples of the anionic emulsifier include sodium alkylbenzene sulfonate and sodium polyoxyethylene nonylphenyl ether sulfate. Among these, sulfonic acid-based emulsifiers such as sodium alkylbenzene sulfonate and sodium lauryl sulfonate are particularly preferable. These emulsifiers are used in the range of about 0.05 to 5 parts by mass with respect to 100 parts by mass (as solid content) of the siloxane mixture.

酸触媒としては、脂肪族スルホン酸、脂肪族置換ベンゼンスルホン酸、脂肪族置換ナフタレンスルホン酸などのスルホン酸類および硫酸、塩酸、硝酸などの鉱酸類が挙げられる。これらの酸触媒は、1種でまたは2種以上を組み合わせて使用できる。これらの中でも、ポリオルガノシロキサンの水性分散体の安定化作用に優れているため、脂肪族置換ベンゼンスルホン酸が好ましく、n−ドデシルベンゼンスルホン酸が特に好ましい。また、n−ドデシルベンゼンスルホン酸と硫酸などの鉱酸とを併用すると、ポリオルガノシロキサンの水性分散体に使用した乳化剤が、熱可塑性樹脂組成物の発色性に影響を及ぼすことを極力抑えることができる。   Examples of the acid catalyst include sulfonic acids such as aliphatic sulfonic acid, aliphatic substituted benzenesulfonic acid, and aliphatic substituted naphthalenesulfonic acid, and mineral acids such as sulfuric acid, hydrochloric acid, and nitric acid. These acid catalysts can be used alone or in combination of two or more. Among these, aliphatic substituted benzenesulfonic acid is preferable, and n-dodecylbenzenesulfonic acid is particularly preferable because it is excellent in the stabilizing action of the aqueous dispersion of polyorganosiloxane. In addition, when n-dodecylbenzenesulfonic acid and a mineral acid such as sulfuric acid are used in combination, the emulsifier used in the aqueous dispersion of polyorganosiloxane can suppress the color development of the thermoplastic resin composition as much as possible. it can.

ジエン系−アクリル系複合ゴム状重合体、シリコーン系−アクリル系複合ゴム状重合体等の複合ゴムの製造方法は、特に制限されない。例えば、アクリル系ゴム状重合体の水性分散体と他のゴム成分の水性分散体とをヘテロ凝集または共肥大化する方法;アクリル系ゴム状重合体の水性分散体または他のゴム成分水性分散体のいずれか一方の存在下で他方を構成する単量体成分を重合させて複合化させる方法等が挙げられる。例えば、ジエン系ゴム状重合体またはシリコーン系ゴム状重合体の存在下で、(メタ)アクリル酸エステルと、架橋剤およびグラフト交叉剤のいずれか一方または両方とを含む単量体成分を乳化重合することにより、ジエン系−アクリル系複合ゴム状重合体またはシリコーン系−アクリル系複合ゴム状重合体が得られる。   The method for producing a composite rubber such as a diene-acrylic composite rubbery polymer or a silicone-acrylic composite rubbery polymer is not particularly limited. For example, a method of heteroaggregating or co-enlarging an aqueous dispersion of an acrylic rubbery polymer and an aqueous dispersion of another rubber component; an aqueous dispersion of an acrylic rubbery polymer or an aqueous dispersion of another rubber component And a method of polymerizing a monomer component constituting the other in the presence of either of them to form a composite. For example, in the presence of a diene rubber-like polymer or silicone rubber-like polymer, a monomer component containing (meth) acrylic acid ester and one or both of a crosslinking agent and a graft crossing agent is emulsion-polymerized. By doing so, a diene-acrylic composite rubbery polymer or a silicone-acrylic composite rubbery polymer is obtained.

<ビニル系単量体成分(m2)>
ビニル系単量体成分(m2)は、少なくとも芳香族ビニル化合物およびシアン化ビニル化合物を含むことが好ましい。ビニル系単量体成分(m2)は、芳香族ビニル化合物およびシアン化ビニル化合物の他に、これらと共重合可能な他の単量体を、本発明の効果を損なわない範囲で含んでもよい。
<Vinyl monomer component (m2)>
The vinyl monomer component (m2) preferably contains at least an aromatic vinyl compound and a vinyl cyanide compound. In addition to the aromatic vinyl compound and the vinyl cyanide compound, the vinyl monomer component (m2) may contain other monomers copolymerizable therewith within a range not impairing the effects of the present invention.

芳香族ビニル化合物としては、例えば、スチレン、α−メチルスチレン、o−,m−またはp−メチルスチレン、ビニルキシレン、p−t−ブチルスチレン、エチルスチレン等が挙げられ、熱可塑性樹脂組成物の流動性、成形品の発色性、耐衝撃性の点から、スチレン、α−メチルスチレンが好ましい。芳香族ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the aromatic vinyl compound include styrene, α-methyl styrene, o-, m- or p-methyl styrene, vinyl xylene, pt-butyl styrene, ethyl styrene, and the like. Styrene and α-methylstyrene are preferable from the viewpoints of fluidity, color developability of molded products, and impact resistance. An aromatic vinyl compound may be used individually by 1 type, and may be used in combination of 2 or more type.

芳香族ビニル化合物の含有率は、ビニル系単量体成分(m2)100質量%中65〜82質量%が好ましく、73〜80質量%がより好ましく、75〜80質量%がさらに好ましい。芳香族ビニル化合物の含有率が前記範囲内であれば、成形品の発色性、耐衝撃性がさらに優れる。   65-82 mass% is preferable in 100 mass% of vinyl-type monomer components (m2), and the content rate of an aromatic vinyl compound has more preferable 73-80 mass%, and 75-80 mass% is further more preferable. When the content of the aromatic vinyl compound is within the above range, the color developability and impact resistance of the molded product are further improved.

シアン化ビニル化合物としては、例えば、アクリロニトリル、メタクリロニトリル等が挙げられる。シアン化ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the vinyl cyanide compound include acrylonitrile and methacrylonitrile. A vinyl cyanide compound may be used individually by 1 type, and may be used in combination of 2 or more type.

シアン化ビニル化合物の含有率は、ビニル系単量体成分(m2)100質量%中18〜35質量%が好ましく、20〜27質量%がより好ましく、20〜25質量%がさらに好ましい。シアン化ビニル化合物の含有率が前記範囲内であれば、成形品の発色性、耐衝撃性がさらに優れる。   The content of the vinyl cyanide compound is preferably 18 to 35% by mass, more preferably 20 to 27% by mass, and further preferably 20 to 25% by mass in 100% by mass of the vinyl monomer component (m2). When the content of the vinyl cyanide compound is within the above range, the color developability and impact resistance of the molded product are further improved.

他の単量体としては、例えば、メタクリル酸エステル(メタクリル酸メチル、メタクリル酸エチル、メタクリル酸n−プロピル、メタクリル酸i−プロピル、メタクリル酸n−ブチル、メタクリル酸i−ブチル、メタクリル酸t−ブチル、メタクリル酸アミル、メタクリル酸イソアミル、メタクリル酸オクチル、メタクリル酸−2−エチルヘキシル、メタクリル酸デシル、メタクリル酸ラウリル、メタクリル酸シクロヘキシル、メタクリル酸ペンジル、メタクリル酸フェニル等)、マレイミド系化合物(N−メチルマレイミド、N−エチルマレイミド、N−n−プロピルマレイミド、N−i−プロピルマレイミド、N−n−ブチルマレイミド、N−i−ブチルマレイミド、N−tert−ブチルマレイミド、N−シクロアルキルマレイミド(N−シクロヘキシルマレイミド等)、N−アリールマレイミド(N−フェニルマレイミド、N−アルキル置換フェニルマレイミド、N−クロロフェニルマレイミド等)、N−アラルキルマレイミド等)、アクリル酸エステル(アクリル酸メチル、アクリル酸エチル、アクリル酸プロピル、アクリル酸ブチル等)等が挙げられる。他の単量体は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Other monomers include, for example, methacrylate esters (methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, i-propyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-methacrylic acid t- Butyl, amyl methacrylate, isoamyl methacrylate, octyl methacrylate, -2-ethylhexyl methacrylate, decyl methacrylate, lauryl methacrylate, cyclohexyl methacrylate, penzyl methacrylate, phenyl methacrylate, etc.), maleimide compounds (N-methyl) Maleimide, N-ethylmaleimide, Nn-propylmaleimide, Ni-propylmaleimide, Nn-butylmaleimide, Ni-butylmaleimide, N-tert-butylmaleimide, N-cycloalkylmaleimide ( -Cyclohexylmaleimide), N-arylmaleimide (N-phenylmaleimide, N-alkyl-substituted phenylmaleimide, N-chlorophenylmaleimide, etc.), N-aralkylmaleimide, etc.), acrylic acid ester (methyl acrylate, ethyl acrylate, acrylic) Propyl acid, butyl acrylate, etc.). Another monomer may be used individually by 1 type and may be used in combination of 2 or more type.

<グラフト共重合体(F)>
グラフト共重合体(F)は、ゴム状重合体(E)の存在下にビニル系単量体成分(m2)を重合することによって得られる。
<Graft copolymer (F)>
The graft copolymer (F) can be obtained by polymerizing the vinyl monomer component (m2) in the presence of the rubber-like polymer (E).

グラフト共重合体(F)は、ゴム状重合体(E)20〜80質量%の存在下に、ビニル系単量体成分(m2)20〜80質量%(ただし、ゴム状重合体(E)とビニル系単量体成分(m2)との合計は100質量%である。)を重合して得られたものが好ましく、ゴム状重合体(E)25〜75質量%の存在下に、ビニル系単量体成分(m2)25〜75質量%を重合して得られたものがより好ましく、ゴム状重合体(E)30〜70質量%の存在下に、ビニル系単量体成分(m2)30〜70質量%を重合して得られたものがさらに好ましい。ゴム状重合体(E)の割合が前記範囲内であれば、グラフト共重合体(F)の生産性が良好であるとともに、成形品の発色性、耐衝撃性がさらに優れる。   The graft copolymer (F) is 20 to 80% by mass of the vinyl monomer component (m2) in the presence of 20 to 80% by mass of the rubbery polymer (E) (however, the rubbery polymer (E) And the vinyl monomer component (m2) is 100% by mass.) And is preferably obtained by polymerizing the rubber-like polymer (E) in the presence of 25 to 75% by mass. What was obtained by polymerizing 25 to 75% by mass of the monomeric monomer component (m2) is more preferable. In the presence of 30 to 70% by mass of the rubber-like polymer (E), the vinyl monomer component (m2) And more preferably obtained by polymerizing 30 to 70% by mass. When the ratio of the rubber-like polymer (E) is within the above range, the productivity of the graft copolymer (F) is good, and the color developability and impact resistance of the molded product are further improved.

グラフト共重合体(F)の重合方法としては、公知の重合方法(乳化重合法、溶液重合法、懸濁重合法、塊状重合法)が挙げられる。
例えば、乳化重合により製造される際、ゴム状重合体(E)の水性分散体にビニル系単量体成分(m2)を加え、乳化剤の存在下でビニル系単量体成分(m2)をラジカル重合させることによりグラフト共重合体(F)の水性分散体が得られる。この際、グラフト率およびグラフト成分の分子量を制御するため、各種公知の連鎖移動剤を添加してもよい。
Examples of the polymerization method of the graft copolymer (F) include known polymerization methods (emulsion polymerization method, solution polymerization method, suspension polymerization method, bulk polymerization method).
For example, when produced by emulsion polymerization, a vinyl monomer component (m2) is added to an aqueous dispersion of a rubber-like polymer (E), and the vinyl monomer component (m2) is radicalized in the presence of an emulsifier. By polymerization, an aqueous dispersion of the graft copolymer (F) is obtained. At this time, various known chain transfer agents may be added in order to control the graft ratio and the molecular weight of the graft component.

ラジカル重合開始剤としては、過酸化物、アゾ系開始剤、酸化剤と還元剤とを組み合わせたレドックス系開始剤等が挙げられ、グラフト重合反応の制御を容易にできる点から、レドックス系開始剤が好ましく、硫酸第一鉄−エチレンジアミン四酢酸二ナトリウム塩−ロンガリット−ヒドロペルオキシドを組み合わせたスルホキシレート系開始剤が特に好ましい。
乳化剤としては、ゴム状重合体(E)の製造の際に用いた乳化剤が挙げられる。ゴム状重合体(E)の水性分散体に含まれる乳化剤をそのまま用い、グラフト重合の際に乳化剤を追加しなくてもよいし、必要に応じてグラフト重合の際に乳化剤を追加してもよい。
Examples of radical polymerization initiators include peroxides, azo-based initiators, redox-based initiators in which an oxidizing agent and a reducing agent are combined, and redox-based initiators from the point that the graft polymerization reaction can be easily controlled. A sulfoxylate-based initiator in which ferrous sulfate-ethylenediaminetetraacetic acid disodium salt-longalite-hydroperoxide is combined is particularly preferable.
As an emulsifier, the emulsifier used in the case of manufacture of a rubber-like polymer (E) is mentioned. The emulsifier contained in the aqueous dispersion of the rubber-like polymer (E) is used as it is, and it is not necessary to add an emulsifier at the time of graft polymerization, or an emulsifier may be added at the time of graft polymerization as necessary. .

グラフト共重合体(F)の水性分散体から、グラフト共重合体(F)を回収する方法としては、凝固剤を溶解させた熱水中に水性分散体を投入して、スラリー状態に凝析することによって回収する方法(湿式法);加熱雰囲気中にグラフト共重合体(F)の水性分散体を噴霧することによって、半直接的にグラフト共重合体(F)を回収する方法(スプレードライ法)等が挙げられる。   As a method for recovering the graft copolymer (F) from the aqueous dispersion of the graft copolymer (F), the aqueous dispersion is poured into hot water in which a coagulant is dissolved, and coagulated in a slurry state. A method of recovering the graft copolymer (F) by spraying an aqueous dispersion of the graft copolymer (F) in a heated atmosphere (spray drying) Law).

凝固剤としては、無機酸(硫酸、塩酸、リン酸、硝酸等)、金属塩(塩化カルシウム、酢酸カルシウム、硫酸アルミニウム等)等が挙げられる。凝固剤は、重合で用いた乳化剤に対応させて選定される。すなわち、乳化剤として脂肪酸のナトリウムまたはカリウム塩、ロジン酸のナトリウムまたはカリウム塩等のカルボン酸のナトリウムまたはカリウム塩のみを用いた場合、どのような凝固剤を用いてもよい。乳化剤としてドデシルベンゼンスルホン酸ナトリウム等の酸性領域でも安定な乳化力を示す乳化剤が含まれている場合、金属塩を用いる必要がある。   Examples of the coagulant include inorganic acids (sulfuric acid, hydrochloric acid, phosphoric acid, nitric acid, etc.), metal salts (calcium chloride, calcium acetate, aluminum sulfate, etc.) and the like. The coagulant is selected according to the emulsifier used in the polymerization. That is, when only a sodium or potassium salt of a carboxylic acid such as a sodium or potassium salt of a fatty acid or a sodium or potassium salt of rosin acid is used as an emulsifier, any coagulant may be used. When an emulsifier exhibiting a stable emulsifying power even in an acidic region such as sodium dodecylbenzenesulfonate is included as an emulsifier, it is necessary to use a metal salt.

スラリー状態のグラフト共重合体(F)から乾燥状態のグラフト共重合体(F)を得る方法としては、洗浄によって、スラリーに残存する乳化剤残渣を水中に溶出させた後に、(i)該スラリーを遠心脱水機またはプレス脱水機で脱水し、さらに気流乾燥機等で乾燥する方法、(ii)圧搾脱水機、押出機等で脱水と乾燥とを同時に実施する方法等が挙げられる。
乾燥後には、グラフト共重合体(F)は、粉体または粒子状で得られる。また、圧搾脱水機または押出機から排出されたグラフト共重合体(F)を直接、熱可塑性樹脂組成物を製造する押出機または成形機に送ってもよい。
As a method for obtaining the dry graft copolymer (F) from the slurry graft copolymer (F), the emulsifier residue remaining in the slurry is eluted in water by washing, and (i) Examples include a method of dehydrating with a centrifugal dehydrator or a press dehydrator and further drying with an air flow dryer or the like, and (ii) a method of simultaneously performing dehydration and drying with a press dehydrator or an extruder.
After drying, the graft copolymer (F) is obtained in the form of powder or particles. Moreover, you may send the graft copolymer (F) discharged | emitted from the press dehydrator or the extruder directly to the extruder or molding machine which manufactures a thermoplastic resin composition.

<ビニル系単量体成分(m3)>
ビニル系単量体成分(m3)は、少なくともメタクリル酸エステルを含む。
ビニル系単量体成分(m3)は、メタクリル酸エステルの他に、マレイミド系化合物、芳香族ビニル化合物、アクリル酸エステル、およびメタクリル酸エステルと共重合可能な他のビニル系単量体の群から選ばれる1種または2種以上の単量体を、本発明の効果を損なわない範囲で含んでもよい。
<Vinyl monomer component (m3)>
The vinyl monomer component (m3) contains at least a methacrylic acid ester.
The vinyl monomer component (m3) includes, in addition to the methacrylic acid ester, a maleimide compound, an aromatic vinyl compound, an acrylic acid ester, and another vinyl monomer copolymerizable with the methacrylic acid ester. One or two or more selected monomers may be included within a range not impairing the effects of the present invention.

メタクリル酸エステルとしては、例えば、メタクリル酸メチル、メタクリル酸エチル、メタクリル酸n−プロピル、メタクリル酸i−プロピル、メタクリル酸n−ブチル、メタクリル酸i−ブチル、メタクリル酸t−ブチル、メタクリル酸アミル、メタクリル酸イソアミル、メタクリル酸オクチル、メタクリル酸−2−エチルヘキシル、メタクリル酸デシル、メタクリル酸ラウリル、メタクリル酸シクロヘキシル、メタクリル酸ペンジル、メタクリル酸フェニル等が挙げられ、成形品の耐熱性および耐衝撃性がさらに優れる点から、メタクリル酸メチルおよびメタクリル酸エチルの少なくとも1種が好ましい。メタクリル酸エステルは、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the methacrylic acid ester include methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, i-propyl methacrylate, n-butyl methacrylate, i-butyl methacrylate, t-butyl methacrylate, amyl methacrylate, Examples include isoamyl methacrylate, octyl methacrylate, -2-ethylhexyl methacrylate, decyl methacrylate, lauryl methacrylate, cyclohexyl methacrylate, penzyl methacrylate, phenyl methacrylate, and the like. From the viewpoint of superiority, at least one of methyl methacrylate and ethyl methacrylate is preferable. A methacrylic acid ester may be used individually by 1 type, and may be used in combination of 2 or more type.

メタクリル酸エステルの含有率は、成形品の耐引っ掻き傷性、発色性の点から、ビニル系単量体成分(m3)100質量%中50〜100質量%が好ましい。   The content of the methacrylic acid ester is preferably 50 to 100% by mass in 100% by mass of the vinyl monomer component (m3) from the viewpoint of scratch resistance and color developability of the molded product.

マレイミド系化合物としては、例えば、N−アルキルマレイミド(N−メチルマレイミド、N−エチルマレイミド、N−n−プロピルマレイミド、N−i−プロピルマレイミド、N−n−ブチルマレイミド、N−i−ブチルマレイミド、N−t−ブチルマレイミド等)、N−シクロアルキルマレイミド(N−シクロヘキシルマレイミド等)、N−アリールマレイミド(N−フェニルマレイミド、N−アルキル置換フェニルマレイミド、N−クロロフェニルマレイミド等)等が挙げられ、成形品の耐熱性および耐衝撃性がさらに優れる点から、N−アリールマレイミドが好ましく、N−フェニルマレイミドが特に好ましい。マレイミド系化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of maleimide compounds include N-alkylmaleimide (N-methylmaleimide, N-ethylmaleimide, Nn-propylmaleimide, Ni-propylmaleimide, Nn-butylmaleimide, Ni-butylmaleimide). , N-t-butylmaleimide, etc.), N-cycloalkylmaleimide (N-cyclohexylmaleimide, etc.), N-arylmaleimide (N-phenylmaleimide, N-alkyl-substituted phenylmaleimide, N-chlorophenylmaleimide, etc.) and the like. From the viewpoint of further improving the heat resistance and impact resistance of the molded product, N-arylmaleimide is preferred, and N-phenylmaleimide is particularly preferred. A maleimide type compound may be used individually by 1 type, and may be used in combination of 2 or more type.

芳香族ビニル化合物としては、例えば、スチレン、α−メチルスチレン、o−,m−またはp−メチルスチレン、ビニルキシレン、p−t−ブチルスチレン、エチルスチレン等が挙げられ、成形品の耐熱性および耐衝撃性がさらに優れる点から、スチレン、α−メチルスチレンが好ましい。芳香族ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the aromatic vinyl compound include styrene, α-methyl styrene, o-, m- or p-methyl styrene, vinyl xylene, pt-butyl styrene, ethyl styrene, and the like. Styrene and α-methylstyrene are preferable from the viewpoint of further excellent impact resistance. An aromatic vinyl compound may be used individually by 1 type, and may be used in combination of 2 or more type.

アクリル酸エステルとしては、例えば、アクリル酸メチル、アクリル酸エチル、アクリル酸プロピル、アクリル酸ブチル等が挙げられ、成形品の耐熱性および耐衝撃性がさらに優れる点から、アクリル酸メチルが好ましい。アクリル酸エステルは、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the acrylate ester include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, and the like, and methyl acrylate is preferred from the viewpoint that the heat resistance and impact resistance of the molded product are further improved. One kind of acrylic acid ester may be used alone, or two or more kinds may be used in combination.

他のビニル系単量体としては、例えば、シアン化ビニル化合物(アクリロニトリル、メタクリロニトリル等)等が挙げられる。他のビニル系単量体は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of other vinyl monomers include vinyl cyanide compounds (acrylonitrile, methacrylonitrile, etc.). Another vinyl-type monomer may be used individually by 1 type, and may be used in combination of 2 or more type.

ビニル系単量体成分(m3)は、メタクリル酸エステルの含有率が50〜94質量%、マレイミド系化合物の含有率が5〜49質量%、芳香族ビニル化合物の含有率が1〜45質量%であることが好ましい。ビニル系単量体成分(m3)100質量%中の各化合物の含有率が前記の範囲内であれば、成形品の耐引っ掻き傷性、発色性、耐衝撃性、耐熱性がさらに優れる。   The vinyl monomer component (m3) has a methacrylic acid ester content of 50 to 94 mass%, a maleimide compound content of 5 to 49 mass%, and an aromatic vinyl compound content of 1 to 45 mass%. It is preferable that When the content of each compound in 100% by mass of the vinyl monomer component (m3) is within the above range, the scratch resistance, color development, impact resistance, and heat resistance of the molded product are further improved.

<メタクリル酸エステル樹脂(G)>
メタクリル酸エステル樹脂(G)は、ビニル系単量体成分(m3)を重合することによって得られる。
重合方法は、限定されない。重合方法としては、公知の重合方法(乳化重合法、懸濁重合法、溶液重合法等)が挙げられる。
<Methacrylate ester resin (G)>
The methacrylic ester resin (G) is obtained by polymerizing the vinyl monomer component (m3).
The polymerization method is not limited. Examples of the polymerization method include known polymerization methods (emulsion polymerization method, suspension polymerization method, solution polymerization method, etc.).

乳化重合法によるメタクリル酸エステル樹脂(G)の製造方法としては、例えば、反応器内にビニル系単量体成分(m3)と乳化剤と重合開始剤と連鎖移動剤とを仕込み、加熱して重合し、メタクリル酸エステル樹脂(G)を含む水性分散体から析出法によってメタクリル酸エステル樹脂(G)を回収する方法が挙げられる。
乳化剤としては、通常の乳化重合用乳化剤(ロジン酸カリウム、アルキルベンゼンスルホン酸ナトリウム等)が挙げられる。
重合開始剤としては、有機、無機の過酸化物系開始剤が挙げられる。
連鎖移動剤としては、メルカプタン類、α−メチルスチレンダイマー、テルペン類等が挙げられる。
析出法としては、水性分散体からグラフト共重合体(D)を回収するときと同様の方法を採用できる。
As a method for producing a methacrylic ester resin (G) by an emulsion polymerization method, for example, a vinyl monomer component (m3), an emulsifier, a polymerization initiator, and a chain transfer agent are charged in a reactor and polymerized by heating. And the method of collect | recovering methacrylic ester resin (G) by the precipitation method from the aqueous dispersion containing methacrylic ester resin (G) is mentioned.
Examples of the emulsifier include usual emulsion polymerization emulsifiers (potassium rosinate, sodium alkylbenzenesulfonate, etc.).
Examples of the polymerization initiator include organic and inorganic peroxide initiators.
Examples of chain transfer agents include mercaptans, α-methylstyrene dimers, terpenes and the like.
As the precipitation method, a method similar to that used when recovering the graft copolymer (D) from the aqueous dispersion can be employed.

懸濁重合法によるメタクリル酸エステル樹脂(G)の製造方法としては、例えば、反応器内にビニル系単量体成分(m3)と懸濁剤と懸濁助剤と重合開始剤と連鎖移動剤とを仕込み、加熱して重合し、スラリーを脱水、乾燥してメタクリル酸エステル樹脂(G)を回収する方法が挙げられる。
懸濁剤としては、トリカルシウムフォスファイト、ポリビニルアルコール等が挙げられる。
懸濁助剤としては、アルキルベンゼンスルホン酸ナトリウム等が挙げられる。
重合開始剤としては、有機ペルオキシド類が挙げられる。
連鎖移動剤としては、メルカプタン類、α−メチルスチレンダイマー、テルペン類等が挙げられる。
Examples of the method for producing a methacrylate ester resin (G) by suspension polymerization include, for example, a vinyl monomer component (m3), a suspending agent, a suspending aid, a polymerization initiator, and a chain transfer agent in a reactor. And heating to polymerize, and the slurry is dehydrated and dried to recover the methacrylic ester resin (G).
Examples of the suspending agent include tricalcium phosphite and polyvinyl alcohol.
Examples of the suspension aid include sodium alkylbenzene sulfonate.
Examples of the polymerization initiator include organic peroxides.
Examples of chain transfer agents include mercaptans, α-methylstyrene dimers, terpenes and the like.

メタクリル酸エステル樹脂(G)は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   A methacrylic ester resin (G) may be used individually by 1 type, and may be used in combination of 2 or more type.

<シリカ粒子(H)>
シリカ粒子(H)を構成するシリカとしては、特に制限はなく、目的に応じて適宜選択でき、例えば、気相法シリカ、結晶性シリカ、溶融シリカなどが挙げられる。
<Silica particles (H)>
There is no restriction | limiting in particular as silica which comprises a silica particle (H), According to the objective, it can select suitably, For example, vapor phase method silica, crystalline silica, fused silica etc. are mentioned.

シリカ粒子(H)の平均粒子径は1〜100nmが好ましく、1〜80nmがより好ましく、1〜50nmがさらに好ましい。シリカ粒子の平均粒子径が上記範囲内であると、得られる成形品の耐傷付き性、発色性が優れる。   The average particle diameter of the silica particles (H) is preferably 1 to 100 nm, more preferably 1 to 80 nm, and further preferably 1 to 50 nm. When the average particle diameter of the silica particles is within the above range, the obtained molded article has excellent scratch resistance and color developability.

シリカ粒子(H)の表面は有機化されていてもよいし、有機化されていなくてもよい。得られる成形品の発色性、耐衝撃性が良好となることから、表面が有機化されていることが好ましい。   The surface of the silica particles (H) may be organically or may not be organically. It is preferable that the surface is made organic because the resulting molded article has good color developability and impact resistance.

シリカ粒子(H)は、求める物性に応じて合成してもいいし、市販のものを使用してもよい。
市販の水性シリカ粒子としては、例えば、スノーテックスOXS(酸性水性シリカゾル、日産化学工業(株)製)、スノーテックスOS(酸性水性シリカゾル、日産化学工業(株)製)、スノーテックスO(酸性水性シリカゾル、日産化学工業(株)製)、スノーテックスO−40(酸性水性シリカゾル、日産化学工業(株)製)、スノーテックスOL(酸性水性シリカゾル、日産化学工業(株)製)、スノーテックスOUP(酸性水性シリカゾル、日産化学工業(株)製)等が挙げられる。
市販の表面が有機化されたシリカ粒子としては、例えば、MEK−ST(メチルエチルケトン分散シリカゾル、日産化学工業(株)製)、MEK−ST−MS(メチルエチルケトン分散シリカゾル、日産化学工業(株)製)、MEK−ST−UP(メチルエチルケトン分散シリカゾル、日産化学工業(株)製)、MIBK−ST(メチルイソブチルケトン分散シリカゾル、日産化学工業(株)製)、EAC−ST(酢酸エチル分散シリカゾル、日産化学工業(株)製)、TOL−ST(トルエン分散シリカゾル、日産化学工業(株)製)、PMA−ST(プロピレンングリコールモノメチルエーテルアセテート分散シリカゾル、日産化学工業(株)製)等が挙げられる。
Silica particles (H) may be synthesized according to the desired physical properties, or commercially available ones may be used.
Examples of commercially available aqueous silica particles include Snowtex OXS (acidic aqueous silica sol, manufactured by Nissan Chemical Industries, Ltd.), Snowtex OS (acidic aqueous silica sol, manufactured by Nissan Chemical Industries, Ltd.), Snowtex O (acidic aqueous solution). Silica sol, manufactured by Nissan Chemical Industries, Ltd., Snowtex O-40 (acidic aqueous silica sol, manufactured by Nissan Chemical Industries, Ltd.), Snowtex OL (acidic aqueous silica sol, manufactured by Nissan Chemical Industries, Ltd.), Snowtex OUP (Acid aqueous silica sol, manufactured by Nissan Chemical Industries, Ltd.).
Examples of commercially available silica particles having an organic surface include MEK-ST (methyl ethyl ketone-dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.), MEK-ST-MS (methyl ethyl ketone-dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.). MEK-ST-UP (methyl ethyl ketone dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.), MIBK-ST (methyl isobutyl ketone dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.), EAC-ST (ethyl acetate dispersed silica sol, Nissan Chemical Co., Ltd.) Kogyo Co., Ltd.), TOL-ST (toluene-dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.), PMA-ST (propylene glycol monomethyl ether acetate-dispersed silica sol, manufactured by Nissan Chemical Industries, Ltd.), and the like.

シリカ粒子の表面を有機化する方法としては、特に制限はなく、公知の方法を採用することができる。例えば、シリカ粒子の表面のシラノール基を有機シラン化合物と反応させて共有結合を形成させることにより有機化する方法、シリカ粒子の表面をラジカル反応性を有するシラン化合物で反応させたのち乳化重合でポリマーをグラフトする方法等が挙げられる。   There is no restriction | limiting in particular as a method of organicizing the surface of a silica particle, A well-known method is employable. For example, a method in which silanol groups on the surface of silica particles are reacted with an organic silane compound to form a covalent bond, and the surface of silica particles is reacted with a radically reactive silane compound and then polymerized by emulsion polymerization. And the like.

シリカ粒子の表面のシラノール基と反応して共有結合を形成することができる有機シラン化合物としては、シラザン化合物、シロキサン化合物、アルコキシシラン、アルコキシシランの部分加水分解物、アルコキシシランの部分加水分解物オリゴマーが挙げられる。有機シラン化合物は、1種を単独で又は2種類以上を混合して用いることができる。   Examples of organosilane compounds that can react with silanol groups on the surface of silica particles to form covalent bonds include silazane compounds, siloxane compounds, alkoxysilanes, alkoxysilane partial hydrolysates, alkoxysilane partial hydrolyzate oligomers. Is mentioned. An organic silane compound can be used individually by 1 type or in mixture of 2 or more types.

シラザン化合物としては、例えば、ヘキサメチルジシラザン、ヘキサエチルジシラザンが挙げられる。
シロキサン化合物としては、例えば、ヘキサメチルジシロキサン、1,3−ジブチルテトラメチルジシロキサン、1,3−ジフェニルテトラメチルジシロキサン、1,3−ジビニルテトラメチルジシロキサン、ヘキサエチルジシロキサン及び3−グリシドキシプロピルペンタメチルジシロキサンが挙げられる。
Examples of the silazane compound include hexamethyldisilazane and hexaethyldisilazane.
Examples of the siloxane compound include hexamethyldisiloxane, 1,3-dibutyltetramethyldisiloxane, 1,3-diphenyltetramethyldisiloxane, 1,3-divinyltetramethyldisiloxane, hexaethyldisiloxane, and 3-glycol. Sidoxypropylpentamethyldisiloxane may be mentioned.

アルコキシシランとしては、例えば、トリメチルメトキシシラン、トリメチルエトキシシラン、トリメチルプロポキシシラン、フェニルジメチルメトキシシラン、クロロプロピルジメチルメトキシシラン、ジメチルジメトキシシラン、メチルトリメトキシシラン、テトラメトキシシラン、テトラエトキシシラン、テトラプロポキシシラン、テトラブトキシシラン、エチルトリメトキシシラン、ジメチルジエトキシシラン、プロピルトリエトキシシラン、n−ブチルトリメトキシシラン、n−ヘキシルトリメトキシシラン、n−オクチルトリエトキシシラン、n−オクチルメチルジエトキシシラン、n−オクタデシルトリメトキシシラン、フェニルトリメトキシシラン、フェニルメチルジメトキシシラン、フェネチルトリメトキシシラン、ドデシルトリメトキシシラン、n−オクタデシルトリエトキシシラン、フェニルジメチルエトキシシラン、フェニルトリエトキシシラン、ジフェニルジメトキシシラン、ビニルトリメトキシシラン、ビニルトリエトキシシラン、ビニルトリス(β−メトキシエトキシ)シラン、γ−メタアクリルオキシプロピルトリメトキシシラン、γ−アクリルオキシプロピルトリメトキシシラン、γ−(メタアクリルオキシプロピル)メチルジメトキシシラン、γ−メタアクリルオキシプロピルメチルジエトキシシラン、γ−メタアクリルオキシプロピルトリエトキシシラン、β−(3,4−エポキシシクロヘキシル)エチルトリメトキシシラン、γ−グリシドキシプロピルトリメトキシシラン、γ−グリシドキシプロピルメチルジエトキシシラン、γ−グリシドキシプロピルトリエトキシシラン、N−(β−アミノエチル)−(γ−アミノプロピル)メチルジメトキシシラン、N−(β−アミノエチル)−(γ−アミノプロピル)トリメトキシシラン、N−(β−アミノエチル)−(γ−アミノプロピル)トリエトキシシラン、γ−アミノプロピルトリメトキシシラン、γ−アミノプロピルトリエトキシシラン、N−フェニル−γ−アミノプロピルトリメトキシシラン、γ−メルカプトプロピルトリメトキシシラン、3−イソシアネートプロピルトリエトキシシラン、トリフルオロプロピルトリメトキシシラン、ヘプタデカトリフルオロプロピルトリメトキシシラン、n−デシルトリメトキシシラン、ジメトキシジエトキシシラン、ビス(トリエトキシシリル)エタン及びヘキサエトキシジシロキサンが挙げられる。   Examples of the alkoxysilane include trimethylmethoxysilane, trimethylethoxysilane, trimethylpropoxysilane, phenyldimethylmethoxysilane, chloropropyldimethylmethoxysilane, dimethyldimethoxysilane, methyltrimethoxysilane, tetramethoxysilane, tetraethoxysilane, and tetrapropoxysilane. , Tetrabutoxysilane, ethyltrimethoxysilane, dimethyldiethoxysilane, propyltriethoxysilane, n-butyltrimethoxysilane, n-hexyltrimethoxysilane, n-octyltriethoxysilane, n-octylmethyldiethoxysilane, n -Octadecyltrimethoxysilane, phenyltrimethoxysilane, phenylmethyldimethoxysilane, phenethyltrimethoxysilane, dode Rutrimethoxysilane, n-octadecyltriethoxysilane, phenyldimethylethoxysilane, phenyltriethoxysilane, diphenyldimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, vinyltris (β-methoxyethoxy) silane, γ-methacryloxypropyl Trimethoxysilane, γ-acryloxypropyltrimethoxysilane, γ- (methacryloxypropyl) methyldimethoxysilane, γ-methacryloxypropylmethyldiethoxysilane, γ-methacryloxypropyltriethoxysilane, β- (3 , 4-epoxycyclohexyl) ethyltrimethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropylmethyldiethoxysilane, γ-glycidoxy Propyltriethoxysilane, N- (β-aminoethyl)-(γ-aminopropyl) methyldimethoxysilane, N- (β-aminoethyl)-(γ-aminopropyl) trimethoxysilane, N- (β-aminoethyl) )-(Γ-aminopropyl) triethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, N-phenyl-γ-aminopropyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, 3- Isocyanatopropyltriethoxysilane, trifluoropropyltrimethoxysilane, heptadecatrifluoropropyltrimethoxysilane, n-decyltrimethoxysilane, dimethoxydiethoxysilane, bis (triethoxysilyl) ethane and hexaethoxydisiloxane .

シリカ粒子の表面の有機化に用いる有機シラン化合物の使用量は、シリカ粒子100質量部に対して0.05〜20質量部が好ましく、0.1〜10質量部がより好ましい。有機シラン化合物の使用量が上記範囲内であれば、シリカ粒子の表面を十分に有機化することができて成形品の発色性が良好となる。   0.05-20 mass parts is preferable with respect to 100 mass parts of silica particles, and, as for the usage-amount of the organosilane compound used for organicization of the surface of a silica particle, 0.1-10 mass parts is more preferable. When the amount of the organic silane compound used is within the above range, the surface of the silica particles can be sufficiently organic, and the color development of the molded product becomes good.

<ビニル系単量体成分(m4)>
ビニル系単量体成分(m4)は、少なくとも芳香族ビニル化合物およびシアン化ビニル化合物を含む。
<Vinyl monomer component (m4)>
The vinyl monomer component (m4) contains at least an aromatic vinyl compound and a vinyl cyanide compound.

芳香族ビニル化合物としては、例えば、スチレン、α−メチルスチレン、o−,m−またはp−メチルスチレン、ビニルキシレン、p−t−ブチルスチレン、エチルスチレン等が挙げられ、熱可塑性樹脂組成物の流動性、成形品の発色性、耐衝撃性の点から、スチレン、α−メチルスチレンが好ましい。芳香族ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the aromatic vinyl compound include styrene, α-methyl styrene, o-, m- or p-methyl styrene, vinyl xylene, pt-butyl styrene, ethyl styrene, and the like. Styrene and α-methylstyrene are preferable from the viewpoints of fluidity, color developability of molded products, and impact resistance. An aromatic vinyl compound may be used individually by 1 type, and may be used in combination of 2 or more type.

芳香族ビニル化合物の含有率は、ビニル系単量体成分(m4)100質量%中15〜95質量%が好ましい。芳香族ビニル化合物の含有率が前記範囲内であれば、成形品の耐衝撃性がさらに向上する。   The content of the aromatic vinyl compound is preferably 15 to 95% by mass in 100% by mass of the vinyl monomer component (m4). When the content of the aromatic vinyl compound is within the above range, the impact resistance of the molded product is further improved.

シアン化ビニル化合物としては、例えば、アクリロニトリル、メタクリロニトリル等が挙げられる。シアン化ビニル化合物は、1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。   Examples of the vinyl cyanide compound include acrylonitrile and methacrylonitrile. A vinyl cyanide compound may be used individually by 1 type, and may be used in combination of 2 or more type.

シアン化ビニル化合物の含有率は、ビニル系単量体成分(m4)100質量%中5〜85質量%が好ましい。シアン化ビニル化合物の含有率が前記範囲内であれば、成形品の耐衝撃性がさらに向上する。   The content of the vinyl cyanide compound is preferably 5 to 85% by mass in 100% by mass of the vinyl monomer component (m4). When the content of the vinyl cyanide compound is within the above range, the impact resistance of the molded product is further improved.

ビニル系単量体成分(m4)は、必要に応じて、メタクリル酸エステル、マレイミド系化合物を含んでいてもよい。
メタクリル酸エステル、マレイミド系化合物としては、ビニル系単量体成分(m3)において例示したものが挙げられる。
The vinyl monomer component (m4) may contain a methacrylic acid ester and a maleimide compound as necessary.
Examples of the methacrylic acid ester and the maleimide compound include those exemplified in the vinyl monomer component (m3).

<スチレン系共重合体(I)>
スチレン系共重合体(I)は、ビニル系単量体成分(m4)を重合して得られる。
重合方法は、限定されない。重合方法としては、公知の重合方法(乳化重合法、懸濁重合法、塊状重合法、溶液重合法等)が挙げられ、成形品の耐熱性の点から、懸濁重合法、塊状重合法が好ましい。
<Styrene copolymer (I)>
The styrene copolymer (I) is obtained by polymerizing the vinyl monomer component (m4).
The polymerization method is not limited. Examples of the polymerization method include known polymerization methods (emulsion polymerization method, suspension polymerization method, bulk polymerization method, solution polymerization method, etc.). From the viewpoint of heat resistance of the molded product, suspension polymerization method and bulk polymerization method are available. preferable.

<他の熱可塑性樹脂>
他の熱可塑性樹脂としては、例えば、ポリカーボネート、ポリブチレンテレフタレート(PBT)、ポリエチレンテレフタレート(PET)、ポリ塩化ビニル、ポリスチレン、ポリアセタール、変性ポリフェニレンエーテル(変性PPE)、エチレン−酢酸ビニル共重合体、ポリアリレート、液晶ポリエステル、ポリエチレン、ポリプロピレン、ポリアミド(ナイロン)等が挙げられる。
<Other thermoplastic resins>
Other thermoplastic resins include, for example, polycarbonate, polybutylene terephthalate (PBT), polyethylene terephthalate (PET), polyvinyl chloride, polystyrene, polyacetal, modified polyphenylene ether (modified PPE), ethylene-vinyl acetate copolymer, poly Examples include arylate, liquid crystal polyester, polyethylene, polypropylene, and polyamide (nylon).

<各種添加剤>
各種添加剤としては、酸化防止剤、滑剤、加工助剤、顔料、充填剤、シリコーンオイル、パラフィンオイル等が挙げられる。
<Various additives>
Examples of various additives include antioxidants, lubricants, processing aids, pigments, fillers, silicone oils, paraffin oils, and the like.

<各成分の含有量>
エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の割合は、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とゴム状重合体(E)との合計(100質量%)のうち、15〜85質量%であり、30〜70質量%が好ましい。
ゴム状重合体(E)の割合は、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とゴム状重合体(E)との合計(100質量%)のうち、85〜15質量%であり、30〜70質量%が好ましい。
エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の割合およびジエン系ゴム状重合体(E)の割合が前記範囲内であれば、少ないゴム含有量で耐衝撃性、耐寒衝撃性を発現することができ、さらに、耐傷付き性、発色性、潤滑性にも優れる。
<Content of each component>
The ratio of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) is the same as that of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer ( Of the total (100% by mass) of C) and the rubbery polymer (E), it is 15 to 85% by mass, preferably 30 to 70% by mass.
The ratio of the rubber-like polymer (E) is the sum of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the rubber-like polymer (E) (100% by mass). ) Is 85 to 15% by mass, preferably 30 to 70% by mass.
If the ratio of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the ratio of the diene rubbery polymer (E) are within the above ranges, the rubber content is small. It can exhibit impact resistance and cold impact resistance, and is excellent in scratch resistance, color development and lubricity.

エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とゴム状重合体(E)との合計の含有量(ゴム含有量)は、熱可塑性樹脂組成物100質量%中5〜30質量%が好ましく、10〜25質量%がより好ましい。ゴム含有量が前記範囲内であれば、熱可塑性樹脂組成物の流動性、成形品の耐衝撃性、耐寒衝撃性、耐傷付き性、発色性、潤滑性がさらに優れる。   The total content (rubber content) of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the rubbery polymer (E) is a thermoplastic resin composition. 5-30 mass% is preferable in 100 mass%, and 10-25 mass% is more preferable. If the rubber content is within the above range, the fluidity of the thermoplastic resin composition, the impact resistance of the molded product, the cold impact resistance, the scratch resistance, the color development and the lubricity are further improved.

グラフト共重合体(D)およびグラフト共重合体(F)の合計の含有量は、グラフト共重合体(D)とグラフト共重合体(F)とメタクリル酸エステル樹脂(G)とスチレン系共重合体(I)との合計100質量%中5〜40質量%が好ましく、10〜30質量%がより好ましい。グラフト共重合体(D)およびグラフト共重合体(F)の合計の含有量が前記範囲内であれば、熱可塑性樹脂組成物の流動性、成形品の耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性、耐熱性等の物性バランスが優れる。   The total content of the graft copolymer (D) and the graft copolymer (F) is as follows: the graft copolymer (D), the graft copolymer (F), the methacrylate ester resin (G), and the styrene copolymer. 5-40 mass% is preferable among 100 mass% in total with coalescence (I), and 10-30 mass% is more preferable. If the total content of the graft copolymer (D) and the graft copolymer (F) is within the above range, the fluidity of the thermoplastic resin composition, the scratch resistance of the molded article, the impact resistance, and the cold impact resistance. Excellent balance of physical properties such as property, color developability, lubricity and heat resistance.

メタクリル酸エステル樹脂(G)の含有量は、グラフト共重合体(D)とグラフト共重合体(F)とメタクリル酸エステル樹脂(G)とスチレン系共重合体(I)との合計100質量%中95〜60質量%が好ましく、90〜70質量%がより好ましい。メタクリル酸エステル樹脂(G)の含有量が前記範囲内であれば、熱可塑性樹脂組成物の流動性、成形品の耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性、耐熱性等の物性バランスが優れる。   The content of the methacrylic ester resin (G) is 100% by mass in total of the graft copolymer (D), the graft copolymer (F), the methacrylic ester resin (G), and the styrene copolymer (I). 95-60 mass% is preferable inside, and 90-70 mass% is more preferable. If the content of the methacrylic ester resin (G) is within the above range, the flowability of the thermoplastic resin composition, scratch resistance of the molded product, impact resistance, cold impact resistance, color development, lubricity, heat resistance Excellent physical property balance.

シリカ粒子(H)の含有量は、グラフト共重合体(D)とグラフト共重合体(F)とメタクリル酸エステル樹脂(G)とスチレン系共重合体(I)との合計100質量部に対し、0.1〜30質量部が好ましく、1〜15質量部がより好ましい。シリカ粒子(H)の含有量が前記範囲の下限値以上であると成形品の耐傷付き性が優れる傾向にあり、前記範囲の上限値以下であると成形品の発色性、耐衝撃性が優れる傾向にある。   The content of the silica particles (H) is 100 parts by mass in total of the graft copolymer (D), the graft copolymer (F), the methacrylic ester resin (G), and the styrene copolymer (I). 0.1-30 mass parts is preferable, and 1-15 mass parts is more preferable. When the content of the silica particles (H) is not less than the lower limit of the above range, the scratch resistance of the molded product tends to be excellent. There is a tendency.

スチレン系共重合体(I)の含有量は、グラフト共重合体(D)とグラフト共重合体(F)とメタクリル酸エステル樹脂(G)とスチレン系共重合体(I)との合計100質量%中0〜40質量%が好ましく、熱可塑性樹脂組成物の流動性、成形品の耐衝撃性、耐寒衝撃性、耐熱性の点から、1〜40質量%がより好ましい。   The total content of the styrene copolymer (I) is 100 masses of the graft copolymer (D), the graft copolymer (F), the methacrylic ester resin (G), and the styrene copolymer (I). % Is preferably 0 to 40% by mass, and more preferably 1 to 40% by mass from the viewpoint of fluidity of the thermoplastic resin composition, impact resistance of the molded article, cold impact resistance, and heat resistance.

<平均粒子径>
熱可塑性樹脂組成物中のグラフト共重合体(D)に含まれるエチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の平均粒子径は0.20〜0.60μmであり、0.30〜0.50μmが好ましい。平均粒子径が0.20μmよりも小さい場合には、成形品の耐衝撃性、耐寒衝撃性が劣る。平均粒子径が0.60μmよりも大きい場合には、成形品の耐衝撃性、耐寒衝撃性、発色性、耐擦り傷性、潤滑性が劣る。エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の平均粒子径が0.30μm〜0.50μmであれば、成形品の耐衝撃性、耐寒衝撃性、発色性、潤滑性、耐擦り傷性がさらに優れる。
<Average particle size>
The average particle size of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) contained in the graft copolymer (D) in the thermoplastic resin composition is 0.20. 0.60 μm, preferably 0.30 to 0.50 μm. When the average particle diameter is smaller than 0.20 μm, the impact resistance and cold impact resistance of the molded product are inferior. When the average particle diameter is larger than 0.60 μm, the molded article is inferior in impact resistance, cold impact resistance, color development, scratch resistance and lubricity. If the average particle diameter of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) is 0.30 μm to 0.50 μm, the impact resistance and cold impact resistance of the molded product Further, color developability, lubricity, and scratch resistance are further improved.

熱可塑性樹脂組成物中のグラフト共重合体(F)に含まれるゴム状重合体(E)の平均粒子径は、0.05〜0.18μmであり、0.07〜0.15μmが好ましい。平均粒子径が0.05μmよりも小さい場合、成形品の耐衝撃性、耐寒衝撃性が劣る。平均粒子径が0.18μmよりも大きい場合、成形品の耐衝撃性、耐寒衝撃性、発色性が劣る。   The average particle diameter of the rubber-like polymer (E) contained in the graft copolymer (F) in the thermoplastic resin composition is 0.05 to 0.18 μm, and preferably 0.07 to 0.15 μm. When the average particle diameter is smaller than 0.05 μm, the impact resistance and cold impact resistance of the molded product are inferior. When the average particle size is larger than 0.18 μm, the impact resistance, cold impact resistance and color developability of the molded product are inferior.

グラフト共重合体(D)が、オレフィン樹脂水性分散体(B)中にてビニル系単量体成分(m1)を重合して得られたものである場合、オレフィン樹脂水性分散体(B)中のエチレン・α−オレフィン共重合体(A)の平均粒子径が、そのまま熱可塑性樹脂組成物中のグラフト共重合体(D)に含まれるエチレン・α−オレフィン共重合体(A)の平均粒子径を示すことを、電子顕微鏡の画像解析によって確認している。
グラフト共重合体(D)が、架橋エチレン・α−オレフィン共重合体(C)の水性分散体中にてビニル系単量体成分(m1)を重合して得られたものである場合、該水性分散体中の架橋エチレン・α−オレフィン共重合体(C)の平均粒子径が、そのまま熱可塑性樹脂組成物中のグラフト共重合体(D)に含まれる架橋エチレン・α−オレフィン共重合体(C)の平均粒子径を示すことを、電子顕微鏡の画像解析によって確認している。
グラフト共重合体(F)が、ゴム状重合体(E)の水性分散体中にてビニル系単量体成分(m2)を重合して得られたものである場合、該水性分散体中のゴム状重合体(E)の平均粒子径が、そのまま熱可塑性樹脂組成物中のグラフト共重合体(F)に含まれるゴム状重合体(E)の平均粒子径を示すことを、電子顕微鏡の画像解析によって確認している。
When the graft copolymer (D) is obtained by polymerizing the vinyl monomer component (m1) in the aqueous olefin resin dispersion (B), the aqueous olefin resin dispersion (B) The average particle diameter of the ethylene / α-olefin copolymer (A) is the average particle size of the ethylene / α-olefin copolymer (A) contained in the graft copolymer (D) in the thermoplastic resin composition as it is. The diameter is confirmed by image analysis using an electron microscope.
When the graft copolymer (D) is obtained by polymerizing the vinyl monomer component (m1) in an aqueous dispersion of the crosslinked ethylene / α-olefin copolymer (C), Crosslinked ethylene / α-olefin copolymer in which the average particle size of the crosslinked ethylene / α-olefin copolymer (C) in the aqueous dispersion is directly included in the graft copolymer (D) in the thermoplastic resin composition It is confirmed by image analysis of an electron microscope that the average particle diameter of (C) is shown.
When the graft copolymer (F) is obtained by polymerizing the vinyl monomer component (m2) in the aqueous dispersion of the rubber-like polymer (E), The average particle diameter of the rubber-like polymer (E) indicates the average particle diameter of the rubber-like polymer (E) contained in the graft copolymer (F) in the thermoplastic resin composition as it is. Confirmed by image analysis.

<熱可塑性樹脂組成物の製造方法>
本発明の熱可塑性樹脂組成物は、グラフト共重合体(D)と、グラフト共重合体(F)と、メタクリル酸エステル樹脂(G)と、シリカ粒子(H)と、必要に応じて他の成分(スチレン系共重合体(I)、他の熱可塑性樹脂、各種添加剤)を混合することにより得られる。
<Method for producing thermoplastic resin composition>
The thermoplastic resin composition of the present invention comprises a graft copolymer (D), a graft copolymer (F), a methacrylic ester resin (G), silica particles (H), and other materials as required. It can be obtained by mixing the components (styrene copolymer (I), other thermoplastic resin, various additives).

熱可塑性樹脂組成物の製造にあたり、各成分を混合する方法としては特に制限はなく、シリカ粒子(H)が熱可塑性樹脂組成物に均一に分散される方法であればよい。例えば、以下の方法(i)〜(iv)等が挙げられる。
(i)グラフト共重合体(D)、グラフト共重合体(F)又はメタクリル酸エステル樹脂(G)の水性分散体を、水媒体のコロイダルシリカとを混合したのちに、無機塩により凝固し、得られた凝固物(シリカ粒子(H)が分散したグラフト共重合体(D)、グラフト共重合体(F)又はメタクリル酸エステル樹脂(G))を回収し、該凝固物と他の成分とを混合する方法。
(ii)有機溶媒に溶解させたメタクリル酸エステル樹脂(G)とシリカ粒子、又は表面が有機化されたシリカ粒子、例えばオルガノシリカゾルとを混合したのちに、有機溶媒を除去して、シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G)を得、該メタクリル酸エステル樹脂(G)と他の成分(グラフト共重合体(D)、グラフト共重合体(F)等)とを混合する方法。
(iii)シリカ粒子、又は表面を有機化されたシリカ粒子、例えば、オルガノシリカゾルの有機溶媒を前述のビニル系単量体成分(m3)に置換したのちに重合して、シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G)を得、該メタクリル酸エステル樹脂(G)と、グラフト共重合体(D)、グラフト共重合体(F)等とを混合する方法。
(iv)ラジカル重合性の有機シラン化合物で処理したシリカ粒子にビニル系単量体成分(m3)をグラフト重合したのち、凝固し、得られた凝固物(シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G))と他の成分(グラフト共重合体(D)、グラフト共重合体(F)等)とを混合する方法。
なかでも、オルガノシリカゾルの有機溶媒をビニル系単量体成分(m3)に置換したのちに懸濁重合することで、シリカ粒子(H)が均一分散したメタクリル酸エステル樹脂(G)を得、このようにシリカ粒子(H)を均一分散状態で含むメタクリル酸エステル樹脂(G)をグラフト共重合体(D)、グラフト共重合体(F)等と混合する方法が、熱可塑性樹脂の生産性、得られる成形品の発色性が良好となることから好ましい。
In the production of the thermoplastic resin composition, the method of mixing each component is not particularly limited, and any method may be used as long as the silica particles (H) are uniformly dispersed in the thermoplastic resin composition. For example, the following methods (i) to (iv) are exemplified.
(I) The aqueous dispersion of the graft copolymer (D), the graft copolymer (F) or the methacrylic ester resin (G) is mixed with colloidal silica as an aqueous medium, and then solidified with an inorganic salt. The obtained coagulated product (graft copolymer (D), graft copolymer (F) or methacrylic ester resin (G) in which silica particles (H) are dispersed) is recovered, and the coagulated product and other components are collected. How to mix.
(Ii) After mixing the methacrylic ester resin (G) dissolved in an organic solvent and silica particles, or silica particles whose surface is organized, for example, organosilica sol, the organic solvent is removed to obtain silica particles ( A method of obtaining a methacrylic ester resin (G) in which H) is dispersed and mixing the methacrylic ester resin (G) with other components (such as a graft copolymer (D) and a graft copolymer (F)). .
(Iii) Silica particles or silica particles whose surface is organized, for example, an organic solvent of an organosilica sol is substituted with the aforementioned vinyl monomer component (m3) and then polymerized to obtain silica particles (H). A method of obtaining a dispersed methacrylic ester resin (G) and mixing the methacrylic ester resin (G) with a graft copolymer (D), a graft copolymer (F) and the like.
(Iv) The vinyl monomer component (m3) is graft-polymerized on silica particles treated with a radical polymerizable organosilane compound, then solidified, and the resulting solidified product (methacrylic acid in which silica particles (H) are dispersed) Ester resin (G)) and other components (graft copolymer (D), graft copolymer (F), etc.) are mixed.
Among these, by replacing the organic solvent of the organosilica sol with the vinyl monomer component (m3) and then performing suspension polymerization, a methacrylate ester resin (G) in which the silica particles (H) are uniformly dispersed is obtained. Thus, the method of mixing the methacrylic ester resin (G) containing the silica particles (H) in a uniformly dispersed state with the graft copolymer (D), the graft copolymer (F), etc., is the productivity of the thermoplastic resin, The resulting molded article is preferable because of good color developability.

<作用効果>
以上説明した本発明の熱可塑性樹脂組成物にあっては、質量平均分子量(Mw)および分子量分布(Mw/Mn)が特定の範囲内にあるエチレン・α−オレフィン共重合体(A)またはこれを架橋処理した架橋エチレン・α−オレフィン共重合体(C)の存在下にビニル系単量体成分(m1)を重合して得られたグラフト共重合体(D)と、ゴム状重合体(E)の存在下にビニル系単量体成分(m2)を重合して得られたグラフト共重合体(F)と、メタクリル酸エステル樹脂(G)と、シリカ粒子(H)とを含み、熱可塑性樹脂組成物中のエチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とジエン系ゴム状重合体(E)とが特定の平均粒子径であり、熱可塑性樹脂組成物中のエチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)とジエン系ゴム状重合体(E)とが特定の割合であるため、流動性が良好であり、また、耐傷付き性、発色性、耐衝撃性、耐寒衝撃性、潤滑性に優れる成形品を得ることができる。また、成形品に耐熱性を付与しても、耐衝撃性を損なうことがない。
<Effect>
In the thermoplastic resin composition of the present invention described above, the ethylene / α-olefin copolymer (A) having a mass average molecular weight (Mw) and a molecular weight distribution (Mw / Mn) within a specific range or this A graft copolymer (D) obtained by polymerizing the vinyl monomer component (m1) in the presence of a crosslinked ethylene / α-olefin copolymer (C) subjected to a crosslinking treatment, and a rubbery polymer ( E) a graft copolymer (F) obtained by polymerizing the vinyl monomer component (m2) in the presence of, a methacrylate ester resin (G), and silica particles (H), The ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the diene rubber-like polymer (E) in the plastic resin composition have a specific average particle diameter, Ethylene α-olefin in thermoplastic resin composition Since the specific ratio of the ethylene copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the diene rubber-like polymer (E) is good, the fluidity is good, and the scratch resistance A molded product excellent in stickiness, color development, impact resistance, cold impact resistance, and lubricity can be obtained. Moreover, even if heat resistance is imparted to the molded article, impact resistance is not impaired.

「成形品」
本発明の成形品は、本発明の熱可塑性樹脂組成物を公知の成形方法によって成形加工して得られる。
成形方法としては、例えば、射出成形法、プレス成形法、押出成形法、真空成形法、ブロー成形法等が挙げられる。
成形品の用途としては、車輌内外装部品、事務機器、家電、建材等が挙げられる。
"Molding"
The molded article of the present invention can be obtained by molding the thermoplastic resin composition of the present invention by a known molding method.
Examples of the molding method include injection molding, press molding, extrusion molding, vacuum molding, and blow molding.
Applications of molded products include vehicle interior / exterior parts, office equipment, home appliances, building materials, and the like.

以上説明した本発明の成形品にあっては、本発明の熱可塑性樹脂組成物を用いているため、耐傷付き性、発色性、耐衝撃性、耐寒衝撃性、潤滑性に優れる。また、メタクリル酸エステル樹脂(G)として特定の共重合組成のものを用いたり、スチレン系共重合体(H)を用いたりすれば、耐熱性にも優れる。   In the molded article of the present invention described above, since the thermoplastic resin composition of the present invention is used, it is excellent in scratch resistance, color development, impact resistance, cold impact resistance, and lubricity. Moreover, if the thing of a specific copolymer composition is used as methacrylic ester resin (G), or a styrene-type copolymer (H) is used, it will be excellent also in heat resistance.

以下、具体的に実施例を示す。ただし、本発明は、これら実施例に限定されるものではない。
以下に記載の「%」は「質量%」、「部」は「質量部」を意味する。
以下の実施例および比較例における各種測定および評価方法は、以下の通りである。
Hereinafter, an example is shown concretely. However, the present invention is not limited to these examples.
In the following, “%” means “mass%” and “part” means “part by mass”.
Various measurements and evaluation methods in the following examples and comparative examples are as follows.

<質量平均分子量(Mw)、分子量分布(Mw/Mn)の測定方法>
GPC(GPC:Waters社製「GPC/V2000」、カラム:昭和電工社製「Shodex AT−G+AT−806MS」)を用い、o−ジクロロベンゼン(145℃)を溶媒として、ポリスチレン換算での質量平均分子量(Mw)、数平均分子量分子量(Mn)を測定し、分子量分布(Mw/Mn)を算出した。
<Measurement Method of Mass Average Molecular Weight (Mw), Molecular Weight Distribution (Mw / Mn)>
Mass average molecular weight in terms of polystyrene using GPC (GPC: “GPC / V2000” manufactured by Waters, column: “Shodex AT-G + AT-806MS” manufactured by Showa Denko KK) and o-dichlorobenzene (145 ° C.) as a solvent. (Mw), number average molecular weight (Mn) were measured, and molecular weight distribution (Mw / Mn) was calculated.

<結晶化度>
理学電機(株)製、広角X線回折装置RAD−RX型を用いて測定したX線回折スペクトルより求めた。
<Crystallinity>
It was determined from an X-ray diffraction spectrum measured using a wide-angle X-ray diffractometer RAD-RX manufactured by Rigaku Corporation.

<平均粒子径の測定方法>
マイクロトラック(日機装社製「ナノトラック150」)を用い、測定溶媒として純水を用いて測定した体積平均粒子径(MV)を平均粒子径とした。
なお、オレフィン樹脂水性分散体(B)に分散しているエチレン・α−オレフィン共重合体(A)や、水性分散体に分散している架橋エチレン・α−オレフィン共重合体(C)や、水性分散体に分散しているゴム状重合体(E)の平均粒子径が、そのまま熱可塑性樹脂組成物中のエチレン・α−オレフィン共重合体(A)や架橋エチレン・α−オレフィン共重合体(C)やゴム状重合体(E)の平均粒子径を示すことを、電子顕微鏡の画像解析によって確認した。
<Measurement method of average particle diameter>
A volume average particle diameter (MV) measured using pure water as a measurement solvent was used as an average particle diameter using Microtrac (“Nanotrack 150” manufactured by Nikkiso Co., Ltd.).
The ethylene / α-olefin copolymer (A) dispersed in the olefin resin aqueous dispersion (B), the crosslinked ethylene / α-olefin copolymer (C) dispersed in the aqueous dispersion, The average particle diameter of the rubber-like polymer (E) dispersed in the aqueous dispersion is the same as the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer in the thermoplastic resin composition. It was confirmed by image analysis with an electron microscope that the average particle diameter of (C) and the rubber-like polymer (E) was shown.

<ゲル含有率の測定方法>
架橋エチレン・α−オレフィン共重合体(C)の水性または溶媒分散体を希硫酸にて凝固させ、水洗、乾燥して得られる凝固粉試料[D1]0.5gを、200mL、110℃のトルエン中に5時間浸漬し、次いで、200メッシュ金網にて濾過し、残渣を乾燥し、その乾燥物[D2]の質量を測定し、下記式(1)から、架橋エチレン・α−オレフィン共重合体(C)のゲル含有率を求めた。
ゲル含有率(%)=乾燥物質量[D2](g)/凝固粉試料質量[D1](g)×100 ・・・(1)
<Measurement method of gel content>
Coagulated powder sample [D1] 0.5 g obtained by coagulating an aqueous or solvent dispersion of the crosslinked ethylene / α-olefin copolymer (C) with dilute sulfuric acid, washing with water, and drying is 200 mL, 110 ° C. toluene. 5 hours, and then filtered through a 200 mesh wire mesh, the residue is dried, the mass of the dried product [D2] is measured, and from the following formula (1), a crosslinked ethylene / α-olefin copolymer The gel content of (C) was determined.
Gel content rate (%) = dry substance amount [D2] (g) / coagulated powder sample mass [D1] (g) × 100 (1)

<溶融混練1>
グラフト共重合体(D)、グラフト共重合体(F)、メタクリル酸エステル樹脂(G)、シリカ粒子(H)、必要に応じて他の成分を混合し、30mmφの真空ベント付き2軸押出機(池貝社製「PCM30」)で、シリンダー温度200〜260℃、93.325kPa真空にて溶融混練を行い、熱可塑性樹脂組成物(1)を得た。さらに、溶融混練後に、ペレタイザー(創研社製「SH型ペレタイザー」)を用いてペレット化を行った。
<Melt-kneading 1>
Graft copolymer (D), graft copolymer (F), methacrylic ester resin (G), silica particles (H), and other components as required are mixed, and a twin screw extruder with a 30 mmφ vacuum vent (PCM30 manufactured by Ikegai Co., Ltd.) was subjected to melt kneading at a cylinder temperature of 200 to 260 ° C. and a vacuum of 93.325 kPa to obtain a thermoplastic resin composition (1). Further, after melt-kneading, pelletization was performed using a pelletizer (“SH type pelletizer” manufactured by Souken Co., Ltd.).

<溶融混練2>
グラフト共重合体(D)、グラフト共重合体(F)、メタクリル酸エステル樹脂(G)、必要に応じて他の成分を混合した合計量100部に対して、シリカ粒子(H)、カーボンブラック0.8部を混合し、30mmφの真空ベント付き2軸押出機(池貝社製「PCM30」)で、シリンダー温度200〜260℃、93.325kPa真空にて溶融混練を行い、熱可塑性樹脂組成物(2)を得た。さらに、溶融混練後に、ペレタイザー(創研社製「SH型ペレタイザー」)を用いてペレット化を行った。
<Melting and kneading 2>
Graft copolymer (D), graft copolymer (F), methacrylic ester resin (G), silica particles (H), carbon black with respect to a total amount of 100 parts mixed with other components as required 0.8 parts are mixed and melt kneaded at a cylinder temperature of 200 to 260 ° C. and a vacuum of 93.325 kPa with a twin screw extruder with a 30 mmφ vacuum vent (“PCM30” manufactured by Ikegai Co., Ltd.), and a thermoplastic resin composition (2) was obtained. Further, after melt-kneading, pelletization was performed using a pelletizer (“SH type pelletizer” manufactured by Souken Co., Ltd.).

<メルトボリュームレート(MVR)の測定>
熱可塑性樹脂組成物(1)について、ISO1133:2011にしたがい、MVRを測定した。なお、MVRは熱可塑性樹脂組成物の流動性の目安となる。
<Measurement of melt volume rate (MVR)>
With respect to the thermoplastic resin composition (1), MVR was measured in accordance with ISO 1133: 2011. In addition, MVR becomes a standard of the fluidity | liquidity of a thermoplastic resin composition.

<射出成形1>
熱可塑性樹脂組成物(1)のペレットを射出成型機(東芝機械社製、「IS55FP−1.5A」)によりシリンダー温度200〜270℃、金型温度60℃の条件で成形し、縦80mm、横10mm、厚さ4mmの成形品を得た。得られた成形品(成形品(Ma1))をシャルピー衝撃試験用成形品、荷重たわみ温度測定用成形品として用いた。
<Injection molding 1>
The pellets of the thermoplastic resin composition (1) were molded by an injection molding machine (Toshiba Machine Co., Ltd., “IS55FP-1.5A”) under the conditions of a cylinder temperature of 200 to 270 ° C. and a mold temperature of 60 ° C. A molded product having a width of 10 mm and a thickness of 4 mm was obtained. The obtained molded product (molded product (Ma1)) was used as a molded product for Charpy impact test and a molded product for measuring deflection temperature under load.

<射出成形2>
熱可塑性樹脂組成物(2)のペレットを射出成型機(東芝機械社製、「IS55FP−1.5A」)によりシリンダー温度200〜270℃、金型温度60℃の条件で成形し、縦100mm、横100mm、厚さ3mmの成形品を得た。得られた成形品(成形品(Ma2))を落球衝撃試験用成形品、発色性評価用成形品、耐引っ掻き傷性評価用成形品、耐擦り傷性評価用成形品、耐候性評価用成形品として用いた。
<Injection molding 2>
The pellets of the thermoplastic resin composition (2) were molded by an injection molding machine (Toshiba Machine Co., Ltd., “IS55FP-1.5A”) under the conditions of a cylinder temperature of 200 to 270 ° C. and a mold temperature of 60 ° C. A molded product having a width of 100 mm and a thickness of 3 mm was obtained. The obtained molded product (molded product (Ma2)) is molded into a falling ball impact test, molded product for evaluation of color development, molded product for evaluation of scratch resistance, molded product for evaluation of scratch resistance, molded product for weather resistance evaluation. Used as.

<射出成形3>
熱可塑性樹脂組成物(1)のペレットを射出成形機(住友重機工業製「SG150−SYCAPM IV」)によってシリンダー温度200〜260℃、金型温度60℃の条件で成形し、図2に示す構造の成形品(試験片21および試験片22)を得た。得られた成形品(成形品(Ma3))を潤滑性評価用成形品として用いた。
<Injection molding 3>
The pellets of the thermoplastic resin composition (1) are molded by an injection molding machine (“SG150-SYCAPM IV” manufactured by Sumitomo Heavy Industries, Ltd.) under conditions of a cylinder temperature of 200 to 260 ° C. and a mold temperature of 60 ° C., and the structure shown in FIG. Molded articles (test piece 21 and test piece 22) were obtained. The obtained molded product (molded product (Ma3)) was used as a molded product for evaluating lubricity.

<耐衝撃性の評価:シャルピー衝撃試験>
成形品(Ma1)について、ISO179−1:2010にしたがい、23℃の条件でシャルピー衝撃試験(ノッチ付)を行い、シャルピー衝撃強度を測定した。
<Evaluation of impact resistance: Charpy impact test>
The molded product (Ma1) was subjected to a Charpy impact test (notched) at 23 ° C. in accordance with ISO 179-1: 2010, and the Charpy impact strength was measured.

<耐寒衝撃性の評価:落球衝撃試験>
−30℃に温調した成形品(Ma2)について、以下の手順で落球衝撃強度を測定した。重さ230gの鋼球を10cmの高さから成形品(Ma2)に落下させ、割れなければ10cm毎に落下高さを高くして割れや亀裂発生の有無を確認した。割れや亀裂が3枚以上発生した落下高さから10cmを除した高さを耐寒落球衝撃高さとし、耐寒落球衝撃高さが50cm以上のとき耐寒落球衝撃性に優れると判定した。
<Evaluation of cold shock resistance: falling ball impact test>
About the molded article (Ma2) temperature-controlled at -30 degreeC, the falling ball impact strength was measured in the following procedures. A steel ball having a weight of 230 g was dropped from a height of 10 cm onto a molded product (Ma2), and if it was not broken, the drop height was increased every 10 cm to confirm whether cracks or cracks occurred. The height obtained by subtracting 10 cm from the drop height at which three or more cracks or cracks occurred was taken as the cold ball impact resistance.

<耐熱性の評価>
成形品(Ma1)について、ISO75:2004に準拠し、1.83MPa、4mm、フラットワイズ法で荷重たわみ温度(℃)を測定した。
<Evaluation of heat resistance>
With respect to the molded article (Ma1), the deflection temperature under load (° C.) was measured by a flatwise method in accordance with ISO 75: 2004, 1.83 MPa, 4 mm.

<発色性の評価>
成形品(Ma2)について、分光測色計(コニカミノルタオプティプス社製「CM−3500d」)を用いて明度Lを、SCE方式にて測定した。こうして測定されたLを「L(ma)」とする。Lが低いほど黒色となり、発色性が良好と判定した。
<Evaluation of color development>
For the molded product (Ma2), the lightness L * was measured by the SCE method using a spectrocolorimeter (“CM-3500d” manufactured by Konica Minolta Optips). The L * measured in this way is referred to as “L * (ma)”. The lower L * was, the more black the color was determined.

<耐引っ掻き傷性の評価>
鉛筆硬度試験機を用い、7.35Nの荷重で、3Hの硬度の鉛筆を成形品(Ma2)の表面に押しつけ、その状態で成形品(Ma2)を5cmほど移動させることによって、成形品(Ma2)の表面を鉛筆で引っ掻き、成形品(Ma2)に傷を付けた。傷を付けた成形品(Mb)の表面の明度Lを、分光測色計を用いて、SCE方式にて測定した。こうして測定されたLを「L(mb)」とする。
上記の結果から、成形品(Mb)の傷の目立ちやすさの判定指標ΔLを下記式(3)から算出した。ΔL(mb−ma)の絶対値が大きいほど傷が目立ちやすい。
ΔL(mb−ma)=L(mb)−L(ma) ・・・(3)
ΔL(mb−ma)の絶対値が1以下のとき、傷が目立たず、成形品の意匠性を損なわない。
ΔL(mb−ma)の絶対値が1.0超〜1.5以下のとき、傷は目立ちにくく、成形品の意匠性を損なわない。
ΔL(mb−ma)の絶対値が1.5超のとき、傷が目立ち、成形品の意匠性を損なう。
<Evaluation of scratch resistance>
Using a pencil hardness tester, a pencil with a hardness of 3H is pressed against the surface of the molded product (Ma2) with a load of 7.35 N, and the molded product (Ma2) is moved about 5 cm in this state, thereby moving the molded product (Ma2). ) Was scratched with a pencil to scratch the molded product (Ma2). The brightness L * of the surface of the scratched molded article (Mb) was measured by the SCE method using a spectrocolorimeter. The L * measured in this way is referred to as “L * (mb)”.
From the above results, a determination index ΔL * for the visibility of scratches on the molded product (Mb) was calculated from the following formula (3). As the absolute value of ΔL * (mb−ma) is larger, the scratches are more conspicuous.
ΔL * (mb−ma) = L * (mb) −L * (ma) (3)
When the absolute value of ΔL * (mb−ma) is 1 or less, scratches are not noticeable and the design of the molded product is not impaired.
When the absolute value of ΔL * (mb−ma) is more than 1.0 to 1.5 or less, scratches are hardly noticeable and the design of the molded product is not impaired.
When the absolute value of ΔL * (mb−ma) is more than 1.5, scratches are conspicuous and the design of the molded product is impaired.

<耐擦り傷性の評価>
図1に示すように、先端部11が半球形に形成された棒状の治具10を用意し、先端部11に、ガーゼを8枚重ねた積層シート12を被せた。成形品(Ma2)13の表面に対して、棒状の治具10が直角になるように、積層シート12が被せられた先端部11を接触させ、先端部11を成形品(Ma2)13の表面において水平方向(図中矢印方向)に摺動させ、100回往復させた。その際、加える荷重は9.8Nとした。100回往復させた後、傷を付けた成形品(Mc)の表面の明度Lを、分光測色計を用いて、SCE方式にて測定した。こうして測定されたLを「L(mc)」とする。
上記の結果から、成形品(Mc)の傷の目立ちやすさの判定指標ΔLを下記式(4)から算出した。ΔL(mc−ma)の絶対値が大きいほど傷が目立ちやすい。
ΔL(mc−ma)=L(mc)−L(ma)・・・(4)
ΔL(mc−ma)の絶対値が3.0未満のとき、傷が目立たず、成形品の意匠性を損なわない。
ΔL(mc−ma)の絶対値が3.0以上〜7.0以下のとき、傷は目立ちにくく、成形品の意匠性を損なわない。
ΔL(mc−ma)の絶対値が7.0超のとき、傷が目立ち、成形品の意匠性を損なう。
<Evaluation of scratch resistance>
As shown in FIG. 1, a rod-like jig 10 having a tip portion 11 formed in a hemispherical shape was prepared, and the tip portion 11 was covered with a laminated sheet 12 in which eight sheets of gauze were stacked. The tip portion 11 covered with the laminated sheet 12 is brought into contact with the surface of the molded product (Ma2) 13 so that the rod-shaped jig 10 is at a right angle, and the tip portion 11 is brought into contact with the surface of the molded product (Ma2) 13. Were slid in the horizontal direction (arrow direction in the figure) and reciprocated 100 times. At that time, the applied load was 9.8 N. After reciprocating 100 times, the lightness L * of the surface of the scratched molded article (Mc) was measured by the SCE method using a spectrocolorimeter. The L * measured in this way is referred to as “L * (mc)”.
From the above results, a determination index ΔL * for the visibility of scratches on the molded product (Mc) was calculated from the following equation (4). As the absolute value of ΔL * (mc−ma) is larger, scratches are more conspicuous.
ΔL * (mc−ma) = L * (mc) −L * (ma) (4)
When the absolute value of ΔL * (mc-ma) is less than 3.0, scratches are not noticeable and the design of the molded product is not impaired.
When the absolute value of ΔL * (mc−ma) is 3.0 or more and 7.0 or less, scratches are not noticeable and the design of the molded product is not impaired.
When the absolute value of ΔL * (mc−ma) is more than 7.0, scratches are conspicuous and the design of the molded product is impaired.

(潤滑性の評価:脱脂前)
成形品(Ma3)において、図2に示すリブ構造21aを有する試験片21および平面部分を有する試験片22を用い、荷重4.9Nまたは9.8Nをかけながら往復運動を行ったときに、きしみ音が発生するか否かを調べた。同様の試験を5回行ったときの、きしみ音の発生と発生した試験回数から、下記基準で評価した。△以上を潤滑性があり、きしみ音の発生抑制効果があるとした。
◎:荷重4.9Nと9.8Nのいずれでもきしみ音が発生しない。
○:荷重9.8Nの場合は小さなきしみ音が発生するが、荷重4.9Nの場合は発生しない。
△:荷重4.9Nと荷重9.8Nのいずれでもきしみ音が発生するが、発生した試験回数がそれぞれの荷重で4回未満である。
×:荷重4.9Nと荷重9.8Nのいずれでもきしみ音が発生し、発生した試験回数がいずれかの荷重で4回以上である。
(Evaluation of lubricity: before degreasing)
In the molded product (Ma3), when the test piece 21 having the rib structure 21a shown in FIG. 2 and the test piece 22 having a flat surface portion are used and a reciprocating motion is performed while applying a load of 4.9N or 9.8N, the squeak is formed. It was investigated whether or not sound was generated. Evaluation was performed based on the following criteria from the occurrence of squeak noise and the number of tests that occurred when the same test was performed five times. Δ or more is considered to have lubricity and to suppress the occurrence of squeak noise.
A: No squeak noise is generated at any load of 4.9N and 9.8N.
○: A small squeak noise is generated when the load is 9.8N, but not when the load is 4.9N.
Δ: A squeak noise is generated at both a load of 4.9 N and a load of 9.8 N, but the number of tests generated is less than 4 at each load.
X: A squeak noise was generated at both a load of 4.9 N and a load of 9.8 N, and the generated number of tests was 4 or more at any load.

(潤滑性の評価:脱脂後)
成形品(Ma3)において、図2に示すリブ構造21aを有する試験片21および平面部分を有する試験片22を60℃にて10日間アニールした後、試験片21および試験片22の表面をイソプロピルアルコールで脱脂することによってブリード成分を取り除いた。脱脂後の基指紋の発生を、脱脂前の潤滑性評価方法と同様にして調べ、下記基準で評価した。△以上を潤滑性の永続性があるとした。
◎:荷重4.9Nと9.8Nのいずれでもきしみ音が発生しない。
○:荷重9.8Nの場合は小さなきしみ音が発生するが、荷重4.9Nの場合は発生しない。
△:荷重4.9Nと荷重9.8Nのいずれでも小さなきしみ音が発生するが、発生した試験回数がそれぞれの荷重で4回未満である。
×:荷重4.9Nと荷重9.8Nのいずれでもきしみ音が発生すし、発生した試験回数がいずれかの荷重で4回以上である。
(Evaluation of lubricity: after degreasing)
In the molded article (Ma3), the test piece 21 having the rib structure 21a shown in FIG. 2 and the test piece 22 having a flat portion are annealed at 60 ° C. for 10 days, and then the surfaces of the test piece 21 and the test piece 22 are isopropyl alcohol. The bleed component was removed by degreasing with. Generation | occurrence | production of the base fingerprint after degreasing was investigated like the lubricity evaluation method before degreasing, and the following reference | standard evaluated. △ or more is regarded as having a permanent lubricity.
A: No squeak noise is generated at any load of 4.9N and 9.8N.
○: A small squeak noise is generated when the load is 9.8N, but not when the load is 4.9N.
Δ: A small squeak noise is generated at both the load 4.9N and the load 9.8N, but the number of tests generated is less than 4 at each load.
X: A squeak noise is generated at both a load of 4.9 N and a load of 9.8 N, and the number of generated tests is 4 or more at any load.

<耐候性の評価>
成形品(Ma2)を、サンシャインウェザーメーター(スガ試験機(株)製)を用い、ブラックパネル温度63℃、サイクル条件60分(降雨12分)の条件で1000時間処理した。そして、その処理前後の変色の度合い(ΔE)を色差計で測定して評価した。ΔEが小さいほど耐候性が良好である。
<Evaluation of weather resistance>
The molded product (Ma2) was treated for 1000 hours under conditions of a black panel temperature of 63 ° C. and a cycle condition of 60 minutes (rainfall of 12 minutes) using a sunshine weather meter (manufactured by Suga Test Instruments Co., Ltd.). Then, the degree of discoloration (ΔE) before and after the treatment was measured with a color difference meter and evaluated. The smaller the ΔE, the better the weather resistance.

<各成分>
以下の例では、下記のエチレン・α−オレフィン共重合体(A)、オレフィン樹脂水性分散体成分(B)、架橋エチレン・α−オレフィン共重合体(C)、グラフト共重合体(D)、グラフト共重合体(F)、メタクリル酸エステル樹脂(G)、フッ素樹脂(H)、スチレン系共重合体(I)を用いた。
<Each component>
In the following examples, the following ethylene / α-olefin copolymer (A), olefin resin aqueous dispersion component (B), crosslinked ethylene / α-olefin copolymer (C), graft copolymer (D), A graft copolymer (F), a methacrylic ester resin (G), a fluororesin (H), and a styrene copolymer (I) were used.

<エチレン・α−オレフィン共重合体(A)>
(エチレン・プロピレン共重合体(A−1)の調製)
20L撹拌機付きステンレス重合槽を十分に窒素置換した後に、脱水精製したヘキサン10Lを添加し、8.0mmol/Lに調製したエチルアルミニウムセスキクロリド(Al(C1.5・Cl1.5)のヘキサン溶液を、5L/hの量で連続的に1時間供給した後、さらに触媒として0.8mmol/Lに調整したVO(OC)Clのヘキサン溶液を5L/hの量で、ヘキサンを5L/hの量で連続的に供給した。一方、重合槽上部から、重合槽内の重合液が常に10Lになるように重合液を連続的に抜き出した。バブリング管を用いてエチレンを2000L/hの量で、プロピレンを1000L/hの量で、水素を9L/hの量で供給し、重合反応を35℃で行った。
前記条件で重合反応を行い、エチレン・プロピレン共重合体(A−1)を含む重合溶液を得た。得られた重合溶液を、塩酸で脱灰した後に、メタノールに投入して析出させた後、乾燥させ、エチレン・プロピレン共重合体(A−1)を得た。エチレン・プロピレン共重合体(A−1)のポリマーの性状を表1に示す。
<Ethylene / α-olefin copolymer (A)>
(Preparation of ethylene / propylene copolymer (A-1))
After fully substituting the stainless polymerization tank equipped with a 20 L stirrer with nitrogen, 10 L of dehydrated and purified hexane was added, and ethylaluminum sesquichloride (Al (C 2 H 5 ) 1.5 · Cl 1 prepared to 8.0 mmol / L was added. 5 ) was continuously supplied at a rate of 5 L / h for 1 hour, and then a hexane solution of VO (OC 2 H 5 ) Cl 2 adjusted to 0.8 mmol / L as a catalyst was further added to 5 L / h. Hexane was continuously fed in an amount of 5 L / h. On the other hand, from the upper part of the polymerization tank, the polymerization liquid was continuously extracted so that the polymerization liquid in the polymerization tank was always 10 L. Using a bubbling tube, ethylene was supplied in an amount of 2000 L / h, propylene was supplied in an amount of 1000 L / h, hydrogen was supplied in an amount of 9 L / h, and a polymerization reaction was performed at 35 ° C.
A polymerization reaction was performed under the above conditions to obtain a polymerization solution containing an ethylene / propylene copolymer (A-1). The obtained polymerization solution was deashed with hydrochloric acid, poured into methanol for precipitation, and then dried to obtain an ethylene / propylene copolymer (A-1). Table 1 shows the properties of the ethylene / propylene copolymer (A-1).

(エチレン・プロピレン共重合体(A−2)〜(A−5)の調製)
表1に示すように水素の供給量を変更した以外は、エチレン・プロピレン共重合体(A−1)と同様にして、エチレン・プロピレン共重合体(A−2)〜(A−5)を得た。エチレン・プロピレン共重合体(A−2)〜(A−5)のポリマーの性状を表1に示す。
(Preparation of ethylene / propylene copolymers (A-2) to (A-5))
Except for changing the hydrogen supply amount as shown in Table 1, the ethylene / propylene copolymers (A-2) to (A-5) were changed in the same manner as the ethylene / propylene copolymer (A-1). Obtained. Table 1 shows the properties of the ethylene / propylene copolymers (A-2) to (A-5).

(エチレン・プロピレン共重合体(A−6)の調製)
20L撹拌機付きステンレス重合槽を十分に窒素置換した後に、脱水精製したヘキサン10Lを添加し、プロピレン110L(標準状態)、水素800mLを添加した。40℃まで加熱した後に、全圧が0.6MPa[gage]となるようにエチレンで加圧した。内圧が0.6MPa[gage]になったところで、トリイソブチルアルミニウム(TIBA)の1.0mM/mLヘキサン溶液10mLを窒素で圧入した。あらかじめ調製しておいた、トリフェニルカルベニウム(テトラキスペンタフルオロフェニル)ボレートをホウ素換算で0.16mM、[ジメチル(t−ブチルアミド)(テトラメチル−η5−シクロペンタジエニル)シラン]チタンクロリドを0.0004mMの量で含むトルエン溶液30mLを、窒素で圧入し重合を開始した。その後、5分間、40℃になるように温度調整し、かつ圧力が0.6MPa[gage]となるようにエチレンの供給を行なった。重合開始5分後、メタノール50mLを挿入して重合を停止し、大気圧まで脱圧し、エチレン・プロピレン共重合体(A−6)を含む重合溶液を得た。得られた重合溶液は、塩酸で脱灰した後に、メタノールに投入して析出させた後、乾燥させ、エチレン・プロピレン共重合体(A−6)を得た。エチレン・プロピレン共重合体(A−6)のポリマーの性状を表1に示す。
(Preparation of ethylene / propylene copolymer (A-6))
After sufficiently substituting a 20 L stainless steel tank with a stirrer with nitrogen, 10 L of dehydrated and purified hexane was added, and 110 L of propylene (standard state) and 800 mL of hydrogen were added. After heating to 40 ° C., it was pressurized with ethylene so that the total pressure was 0.6 MPa [gage]. When the internal pressure reached 0.6 MPa [gage], 10 mL of a 1.0 mM / mL hexane solution of triisobutylaluminum (TIBA) was injected with nitrogen. Triphenylcarbenium (tetrakispentafluorophenyl) borate prepared in advance is 0.16 mM in terms of boron, and [dimethyl (t-butylamide) (tetramethyl-η5-cyclopentadienyl) silane] titanium chloride is 0. Polymerization was initiated by injecting 30 mL of a toluene solution containing 0004 mM with nitrogen. Thereafter, the temperature was adjusted to 40 ° C. for 5 minutes, and ethylene was supplied so that the pressure became 0.6 MPa [gage]. Five minutes after the start of polymerization, 50 mL of methanol was inserted to stop the polymerization, and the pressure was released to atmospheric pressure to obtain a polymerization solution containing an ethylene / propylene copolymer (A-6). The obtained polymerization solution was deashed with hydrochloric acid, poured into methanol for precipitation, and then dried to obtain an ethylene / propylene copolymer (A-6). Table 1 shows the properties of the ethylene / propylene copolymer (A-6).

(エチレン・プロピレン共重合体(A−8)の調製)
触媒としてVO(OC)Clに代えてVClを用いた以外はエチレン・プロピレン共重合体(A−3)と同様にして、エチレン・プロピレン共重合体(A−8)を得た。エチレン・プロピレン共重合体(A−8)のポリマーの性状を表1に示す。
(Preparation of ethylene / propylene copolymer (A-8))
An ethylene / propylene copolymer (A-8) is obtained in the same manner as the ethylene / propylene copolymer (A-3) except that VCl 4 is used instead of VO (OC 2 H 5 ) Cl 2 as a catalyst. It was. Table 1 shows the properties of the ethylene / propylene copolymer (A-8).

(エチレン・プロピレン共重合体(A−7)の調製)
エチレン・プロピレン共重合体(A−3)30部とエチレン・プロピレン共重合体(A−8)70部とを混合し、30mmφの真空ベント付き2軸押出機(池貝社製、「PCM30」)で200℃、93.325kPa真空にて溶融混練し、エチレン・プロピレン共重合体(A−7)を調製した。エチレン・プロピレン共重合体(A−7)のポリマーの性状を表1に示す。
(Preparation of ethylene / propylene copolymer (A-7))
30 parts of ethylene / propylene copolymer (A-3) and 70 parts of ethylene / propylene copolymer (A-8) are mixed, and a 30 mmφ vacuum vented twin screw extruder (“PCM30” manufactured by Ikegai Co., Ltd.) Was melt-kneaded at 200 ° C. and 93.325 kPa vacuum to prepare an ethylene / propylene copolymer (A-7). Table 1 shows the properties of the ethylene / propylene copolymer (A-7).

Figure 0006291702
Figure 0006291702

<オレフィン樹脂水性分散体成分(B)>
(オレフィン樹脂水性分散体(B−1)の調製)
エチレン・プロピレン共重合体(A−1)100部と、酸変性オレフィン重合体として無水マレイン酸変性ポリエチレン(三井化学社製、「三井ハイワックス 2203A」、質量平均分子量:2,700、酸価:30mg/g)20部と、アニオン系乳化剤としてオレイン酸カリウム5部とを混合した。
この混合物を2軸スクリュー押出機(池貝社製、「PCM30」、L/D=40)のホッパーから4kg/hで供給し、該2軸スクリュー押出機のベント部に設けた供給口より、水酸化カリウム0.5部とイオン交換水2.4部を混合した水溶液を連続的に供給しながら、220℃に加熱して溶融混練して押出した。溶融混練物を2軸スクリュー押出機の先端に取り付けた冷却装置に連続的に供給し、90℃まで冷却した。そして、2軸スクリュー押出機先端より吐出させた固体を、80℃の温水中に投入し、連続的に分散させて、固形分濃度40質量%付近まで希釈して、オレフィン樹脂水性分散体(B−1)を得た。オレフィン樹脂水性分散体(B−1)に分散しているエチレン・α−オレフィン共重合体(A)の平均粒子径を表2に示す。
<Olefin resin aqueous dispersion component (B)>
(Preparation of aqueous dispersion of olefin resin (B-1))
100 parts of ethylene / propylene copolymer (A-1) and maleic anhydride-modified polyethylene (manufactured by Mitsui Chemicals, "Mitsui High Wax 2203A") as the acid-modified olefin polymer, mass average molecular weight: 2,700, acid value: 30 mg / g) 20 parts and 5 parts of potassium oleate as an anionic emulsifier were mixed.
This mixture is supplied at 4 kg / h from a hopper of a twin screw extruder (Ikegai, “PCM30”, L / D = 40), and water is supplied from a supply port provided in a vent portion of the twin screw extruder. While continuously supplying an aqueous solution obtained by mixing 0.5 part of potassium oxide and 2.4 parts of ion-exchanged water, it was heated to 220 ° C., melt-kneaded and extruded. The melt-kneaded product was continuously supplied to a cooling device attached to the tip of the twin screw extruder and cooled to 90 ° C. Then, the solid discharged from the tip of the twin screw extruder is poured into warm water at 80 ° C., continuously dispersed, diluted to a solid content concentration of about 40% by mass, and an aqueous olefin resin dispersion (B -1) was obtained. Table 2 shows the average particle diameter of the ethylene / α-olefin copolymer (A) dispersed in the aqueous olefin resin dispersion (B-1).

(オレフィン樹脂水性分散体(B−2)〜(B−8)の調製)
表2に示すように、エチレン・α−オレフィン共重合体(A)として(A−1)を(A−2)〜(A−8)へ変更した以外は、オレフィン樹脂水性分散体(B−1)と同様にして、オレフィン樹脂水性分散体(B−2)〜(B−8)を得た。
各オレフィン樹脂水性分散体(B−2)〜(B−8)に分散しているエチレン・α−オレフィン共重合体(A)の平均粒子径を表2に示す。
(Preparation of aqueous olefin resin dispersions (B-2) to (B-8))
As shown in Table 2, the olefin resin aqueous dispersion (B-) except that (A-1) was changed to (A-2) to (A-8) as the ethylene / α-olefin copolymer (A). In the same manner as in 1), olefin resin aqueous dispersions (B-2) to (B-8) were obtained.
Table 2 shows the average particle size of the ethylene / α-olefin copolymer (A) dispersed in each olefin resin aqueous dispersion (B-2) to (B-8).

(オレフィン樹脂水性分散体(B−9)〜(B−16)の調製)
表3に示すように、乳化する際の水酸化カリウムの添加部数、イオン交換水の添加部数を変更した以外は、オレフィン樹脂水性分散体(B−3)と同様にして、オレフィン樹脂水性分散体(B−9)〜(B−16)を得た。
各オレフィン樹脂水性分散体(B−9)〜(B−16)に分散しているエチレン・α−オレフィン共重合体(A)の平均粒子径を表3に示す。
(Preparation of aqueous olefin resin dispersions (B-9) to (B-16))
As shown in Table 3, the aqueous olefin resin dispersion was the same as the aqueous olefin resin dispersion (B-3) except that the number of added parts of potassium hydroxide during emulsification and the number of added parts of ion exchange water were changed. (B-9) to (B-16) were obtained.
Table 3 shows the average particle size of the ethylene / α-olefin copolymer (A) dispersed in each of the olefin resin aqueous dispersions (B-9) to (B-16).

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

<架橋エチレン・α−オレフィン共重合体(C)>
(架橋エチレン・α−オレフィン共重合体(C−1)の調製)
オレフィン樹脂水性分散体(B−1)(固形分として100部)に、固形分濃度が35%になるようにイオン交換水を加え、有機過酸化物としてt−ブチルクミルペルオキシド1部、多官能性化合物としてジビニルベンゼン1部を添加し、130℃で5時間反応させて、架橋エチレン・α−オレフィン共重合体(C−1)を調製した。架橋エチレン・α−オレフィン共重合体(C−1)のゲル含有率、平均粒子径を表4に示す。
<Crosslinked ethylene / α-olefin copolymer (C)>
(Preparation of crosslinked ethylene / α-olefin copolymer (C-1))
Ion exchange water was added to the olefin resin aqueous dispersion (B-1) (100 parts as a solid content) so that the solid content concentration was 35%, and 1 part of t-butylcumyl peroxide as an organic peroxide was obtained. As a functional compound, 1 part of divinylbenzene was added and reacted at 130 ° C. for 5 hours to prepare a crosslinked ethylene / α-olefin copolymer (C-1). Table 4 shows the gel content and average particle diameter of the crosslinked ethylene / α-olefin copolymer (C-1).

(架橋エチレン・α−オレフィン共重合体(C−2)〜(C−20)の調製)
表4〜6に示すようにオレフィン樹脂水性分散体(B)の種類とt−ブチルクミルペルオキシドの添加量を変更した以外は、架橋エチレン・α−オレフィン共重合体(C−1)と同様にして、架橋エチレン・α−オレフィン共重合体(C−2)〜(C−20)を得た。架橋エチレン・α−オレフィン共重合体(C−2)〜(C−20)のゲル含有率、平均粒子径を表4〜6に示す。
(Preparation of crosslinked ethylene / α-olefin copolymers (C-2) to (C-20))
As shown in Tables 4-6, the same as the crosslinked ethylene / α-olefin copolymer (C-1) except that the type of the olefin resin aqueous dispersion (B) and the amount of t-butylcumyl peroxide added were changed. Thus, crosslinked ethylene / α-olefin copolymers (C-2) to (C-20) were obtained. Tables 4 to 6 show the gel content and average particle size of the crosslinked ethylene / α-olefin copolymers (C-2) to (C-20).

(架橋エチレン・α−オレフィン共重合体(C−21)の調製)
エチレン・α−オレフィン共重合体(A−3)100部に対し、有機過酸化物としてα,α’−ジ(t−ブチルペルオキシ)ジイソプロピルベンゼン0.5部と、ジビニルベンゼン1.0部とを混合し、30mmφの真空ベント付き2軸押出機(池貝社製、「PCM‐30」)で、220℃、93.325kPa真空にて溶融混練を行った後、細かく粉砕することで、架橋エチレン・α−オレフィン共重合体(C−21)を得た。架橋エチレン・α−オレフィン共重合体(C−21)のゲル含有率、平均粒子径を表6に示す。
(Preparation of crosslinked ethylene / α-olefin copolymer (C-21))
With respect to 100 parts of the ethylene / α-olefin copolymer (A-3), 0.5 part of α, α′-di (t-butylperoxy) diisopropylbenzene and 1.0 part of divinylbenzene as an organic peroxide, Are mixed and melt-kneaded at 220 ° C. and 93.325 kPa vacuum in a twin screw extruder with a 30 mmφ vacuum vent (“Ikegai Co., Ltd.,“ PCM-30 ”), and then finely pulverized. -Obtained (alpha) -olefin copolymer (C-21). Table 6 shows the gel content and average particle size of the crosslinked ethylene / α-olefin copolymer (C-21).

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

<グラフト共重合体(D)>
(グラフト共重合体(D−1)の調製)
撹拌機付きステンレス重合槽に、架橋エチレン・α−オレフィン共重合体(C−1)(エチレン・プロピレン共重合体(A−1)の固形分として70部)を入れ、架橋エチレン・α−オレフィン共重合体(C−1)に固形分濃度が30%になるようにイオン交換水を加え、硫酸第一鉄0.006部、ピロリン酸ナトリウム0.3部およびフラクトース0.35部を仕込み、温度を80℃とした。スチレン23.4部、アクリロニトリル6.6部およびクメンヒドロペルオキシド0.6部を150分間連続的に添加し、重合温度を80℃に保ち乳化重合を行った。重合後、グラフト共重合体(D−1)を含む水性分散体に酸化防止剤を添加し、硫酸にて固形分の析出を行い、洗浄、脱水、乾燥の工程を経て、粉状のグラフト共重合体(D−1)を得た。
<Graft copolymer (D)>
(Preparation of graft copolymer (D-1))
In a stainless steel polymerization tank equipped with a stirrer, the crosslinked ethylene / α-olefin copolymer (C-1) (70 parts as a solid content of the ethylene / propylene copolymer (A-1)) is placed, and the crosslinked ethylene / α-olefin is added. Ion exchange water is added to the copolymer (C-1) so that the solid content concentration is 30%, and 0.006 part of ferrous sulfate, 0.3 part of sodium pyrophosphate and 0.35 part of fructose are charged. The temperature was 80 ° C. Styrene (23.4 parts), acrylonitrile (6.6 parts) and cumene hydroperoxide (0.6 parts) were continuously added for 150 minutes, and the polymerization temperature was kept at 80 ° C. to carry out emulsion polymerization. After the polymerization, an antioxidant is added to the aqueous dispersion containing the graft copolymer (D-1), solids are precipitated with sulfuric acid, and after washing, dehydration and drying, A polymer (D-1) was obtained.

(グラフト共重合体(D−2)〜(D−20)の調製)
表7〜9に示すように架橋エチレン・α−オレフィン共重合体(C)の種類を変更した以外は、グラフト共重合体(D−1)と同様にして、グラフト共重合体(D−2)〜(D−20)を得た。
(Preparation of graft copolymers (D-2) to (D-20))
As shown in Tables 7 to 9, the graft copolymer (D-2) was the same as the graft copolymer (D-1) except that the type of the crosslinked ethylene / α-olefin copolymer (C) was changed. ) To (D-20) were obtained.

(グラフト共重合体(D−21)の調製)
撹拌機付きステンレス重合槽に、架橋エチレン・α−オレフィン共重合体(C−21)70部、トルエン300部を仕込み、内容物を70℃で1時間撹拌して均一に溶解した。十分に窒素置換を行った後、スチレン23.4部、アクリロニトリル6.6部、t−ドデシルメルカプタン0.24部、t−ブチルペルオキシイソプロピルモノカーボネート0.22部を添加し、内温を110℃まで昇温し、4時間反応させた。内温を120℃に昇温し、2時間反応させた。重合後、内温を100℃まで冷却し、オクタデシル−3−(3,5−ジ−t−ブチル−4−ヒドロキシフェノール)−プロピオネート0.2部を添加した。反応混合物を抜き出し、水蒸気蒸留によって未反応物と溶媒を留去した。30mmφの真空ベント付き2軸押出機(池貝社製、「PCM30」)で220℃、93.325kPa真空にて、揮発分を実質的に脱揮させ、ペレット化し、グラフト共重合体(D−21)を得た。グラフト共重合体(D−21)のグラフト率を測定したところ26%であった。電子顕微鏡により、グラフト共重合体(D−21)中のエチレン・α−オレフィン共重合体(A)の平均粒子径を確認したところ、0.39μmであった。
(Preparation of graft copolymer (D-21))
In a stainless steel polymerization tank equipped with a stirrer, 70 parts of a crosslinked ethylene / α-olefin copolymer (C-21) and 300 parts of toluene were charged, and the contents were stirred and stirred uniformly at 70 ° C. for 1 hour. After sufficiently purging with nitrogen, 23.4 parts of styrene, 6.6 parts of acrylonitrile, 0.24 parts of t-dodecyl mercaptan and 0.22 parts of t-butylperoxyisopropyl monocarbonate were added, and the internal temperature was 110 ° C. The mixture was heated up to react for 4 hours. The internal temperature was raised to 120 ° C. and reacted for 2 hours. After the polymerization, the internal temperature was cooled to 100 ° C., and 0.2 part of octadecyl-3- (3,5-di-tert-butyl-4-hydroxyphenol) -propionate was added. The reaction mixture was extracted, and unreacted substances and the solvent were distilled off by steam distillation. The volatile matter was substantially devolatilized at 220 ° C. and 93.325 kPa vacuum in a twin screw extruder with a 30 mmφ vacuum vent (“PCM30”, manufactured by Ikegai Co., Ltd.), pelletized, and graft copolymer (D-21). ) The graft ratio of the graft copolymer (D-21) was measured and found to be 26%. When the average particle diameter of the ethylene / α-olefin copolymer (A) in the graft copolymer (D-21) was confirmed by an electron microscope, it was 0.39 μm.

(グラフト共重合体(D−22)の調製)
表9に示すように架橋エチレン・α−オレフィン共重合体(C)をオレフィン樹脂水性分散体(B−3)に変更した以外は、グラフト共重合体(D−1)と同様にして、グラフト共重合体(D−22)を得た。
(Preparation of graft copolymer (D-22))
As shown in Table 9, the grafted ethylene / α-olefin copolymer (C) was changed to an aqueous olefin resin dispersion (B-3), except that the graft copolymer (D-1) was used. A copolymer (D-22) was obtained.

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

<グラフト共重合体(F)>
(グラフト共重合体(F−1)の調製)
オクタメチルシクロテトラシロキサン9 8 部とγ−メタクリロイルオキシプロピルジメトキシメチルシラン2部とを混合してシロキサン系混合物100部を得た。これに、ドデシルベンゼンスルホン酸ナトリウム0.67部と脱イオン水300部からなる水溶液を添加し、ホモミキサーで10000回転/ 分で2分間撹拌した後、ホモジナイザーに20MPaの圧力で1回通し、安定な予備混合オルガノシロキサンラテックスを得た。
一方、試薬注入容器、冷却管、ジャケット加熱器および攪拌装置を備えた反応器内に、ドデシルベンゼンスルホン酸10部、脱イオン水90部を投入し、10%のドデシルベンゼンスルホン酸水溶液を調製した。この水溶液を85℃に加熱した状態で、予備混合したオルガノシロキサンラテックスを4時間にわたって滴下し、滴下終了後1時間その温度を保持した後、40℃以下に冷却した。次いで、この反応物を苛性ソーダ水溶液でpH7に中和し重合を完結することで、ポリオルガノシロキサン(Ea)水性分散体(固形分濃度16.8%)を得た。
<Graft copolymer (F)>
(Preparation of graft copolymer (F-1))
9 parts of octamethylcyclotetrasiloxane and 2 parts of γ-methacryloyloxypropyldimethoxymethylsilane were mixed to obtain 100 parts of a siloxane-based mixture. To this was added an aqueous solution consisting of 0.67 parts of sodium dodecylbenzenesulfonate and 300 parts of deionized water, stirred for 2 minutes at 10000 rpm with a homomixer, and then passed once through the homogenizer at a pressure of 20 MPa. A premixed organosiloxane latex was obtained.
On the other hand, 10 parts of dodecylbenzenesulfonic acid and 90 parts of deionized water were charged into a reactor equipped with a reagent injection container, a cooling tube, a jacket heater, and a stirring device to prepare a 10% aqueous solution of dodecylbenzenesulfonic acid. . While this aqueous solution was heated to 85 ° C., the premixed organosiloxane latex was added dropwise over 4 hours. After the completion of the addition, the temperature was maintained for 1 hour, and then cooled to 40 ° C. or lower. Subsequently, this reaction product was neutralized to pH 7 with an aqueous caustic soda solution to complete the polymerization, whereby an aqueous polyorganosiloxane (Ea) dispersion (solid content concentration 16.8%) was obtained.

次に、試薬注入容器、冷却管、ジャケット加熱器及び撹拌装置を備えた反応器内に、ポリオルガノシロキサン(Ea)水性分散体119.5部、ポリオキシエチレンアルキルフェニルエーテル硫酸ナトリウム0.8部を仕込み、イオン交換水203部を添加し、混合した。その後、n−ブチルアクリレート53.2部、アリルメタクリレート0.21部、1,3−ブチレングリコールジメタクリレート0.11部及びターシャリーブチルハイドロパーオキサイド0.13部からなる混合物を添加した。この反応器に窒素気流を通じることによって、雰囲気の窒素置換を行い、60℃まで昇温した。反応器の内部の温度が60℃になった時点で、硫酸第一鉄0.0001部、エチレンジアミン四酢酸二ナトリウム塩0.0003部及びロンガリット0.24部をイオン交換水10部に溶解させた水溶液を添加し、ラジカル重合を開始させた。アクリレート成分の重合により、液温は78℃まで上昇した。1時間この状態を維持し、アクリレート成分の重合を完結させて、ポリオルガノシロキサン(Ea)と(メタ)アクリル酸エステル系単量体単位と架橋剤および/またはグラフト交叉剤とを含有するポリ(メタ)アクリル酸エステルとからなる複合ゴム状重合体(E−1)の水性分散体を得た。水性分散体に分散している複合ゴム状重合体(E−1)の体積均粒子径は0.08μmであった。
反応器内部の液温が60℃に低下した後、ロンガリット0.4部をイオン交換水10部に溶解した水溶液を添加した。次いで、アクリロニトリル11.1部、スチレン33.2部及びターシャリーブチルハイドロパーオキサイド0.2部の混合液を約1時間にわたって滴下し重合した。滴下終了後1時間保持した後、硫酸第一鉄0.0002部、エチレンジアミン四酢酸二ナトリウム塩0.0006部及びロンガリット0.25部をイオン交換水10部に溶解させた水溶液を添加した。次いで、アクリロニトリル7.4部、スチレン22.2部及びターシャリーブチルハイドロパーオキサイド0.1部の混合液を約40分間にわたって滴下し重合した。滴下終了後1時間保持した後、冷却して、複合ゴム状重合体(E−1)にアクリロニトリル−スチレン共重合体をグラフトさせたグラフト共重合体(F−1)の水性分散体を得た。次いで、酢酸カルシウムを5%の割合で溶解した水溶液150部を60℃に加熱し撹拌した。その酢酸カルシウム水溶液中にグラフト共重合体(F−1)の水性分散体100部を徐々に滴下して凝固させた。得られた凝固物を分離し、洗浄した後、乾燥させて、グラフト共重合体(F−1)の乾燥粉末を得た。
Next, 119.5 parts of an aqueous dispersion of polyorganosiloxane (Ea) and 0.8 part of sodium polyoxyethylene alkylphenyl ether sulfate are placed in a reactor equipped with a reagent injection container, a cooling tube, a jacket heater and a stirring device. Was added, and 203 parts of ion-exchanged water was added and mixed. Thereafter, a mixture consisting of 53.2 parts of n-butyl acrylate, 0.21 part of allyl methacrylate, 0.11 part of 1,3-butylene glycol dimethacrylate and 0.13 part of tertiary butyl hydroperoxide was added. The atmosphere was purged with nitrogen by passing a nitrogen stream through the reactor, and the temperature was raised to 60 ° C. When the temperature inside the reactor reached 60 ° C, 0.0001 part of ferrous sulfate, 0.0003 part of disodium ethylenediaminetetraacetic acid and 0.24 part of Rongalite were dissolved in 10 parts of ion-exchanged water. An aqueous solution was added to initiate radical polymerization. The liquid temperature rose to 78 ° C. by polymerization of the acrylate component. This state is maintained for 1 hour, polymerization of the acrylate component is completed, and poly (siloxane) containing polyorganosiloxane (Ea), a (meth) acrylate monomer unit, a crosslinking agent and / or a graft crossing agent is contained. An aqueous dispersion of a composite rubber-like polymer (E-1) composed of a (meth) acrylic ester was obtained. The volume average particle diameter of the composite rubber-like polymer (E-1) dispersed in the aqueous dispersion was 0.08 μm.
After the liquid temperature inside the reactor dropped to 60 ° C., an aqueous solution in which 0.4 part of Rongalite was dissolved in 10 parts of ion-exchanged water was added. Subsequently, 11.1 parts of acrylonitrile, 33.2 parts of styrene, and 0.2 part of tertiary butyl hydroperoxide were dropped and polymerized over about 1 hour. After holding for 1 hour after the completion of dropping, an aqueous solution in which 0.0002 parts of ferrous sulfate, 0.0006 parts of ethylenediaminetetraacetic acid disodium salt and 0.25 parts of Rongalite were dissolved in 10 parts of ion-exchanged water was added. Next, a mixture of 7.4 parts of acrylonitrile, 22.2 parts of styrene, and 0.1 part of tertiary butyl hydroperoxide was added dropwise over about 40 minutes for polymerization. After holding for 1 hour after the completion of dropping, the mixture was cooled to obtain an aqueous dispersion of a graft copolymer (F-1) obtained by grafting an acrylonitrile-styrene copolymer onto a composite rubber-like polymer (E-1). . Next, 150 parts of an aqueous solution in which calcium acetate was dissolved at a rate of 5% was heated to 60 ° C. and stirred. 100 parts of an aqueous dispersion of the graft copolymer (F-1) was gradually dropped into the calcium acetate aqueous solution to be solidified. The obtained solidified product was separated, washed, and dried to obtain a dry powder of the graft copolymer (F-1).

(グラフト共重合体(F−2)の調製)
試薬注入容器、冷却管、ジャケット加熱器及び撹拌装置を備えた反応器内に、ポリオルガノシロキサン(Ea)水性分散体119.5部、ポリオキシエチレンアルキルフェニルエーテル硫酸ナトリウム0.94部を仕込み、イオン交換水203部を添加し、混合した。その後、n−ブチルアクリレート53.2部、アリルメタクリレート0.21部、1,3−ブチレングリコールジメタクリレート0.11部及びターシャリーブチルハイドロパーオキサイド0.13部からなる混合物を添加した。この反応器に窒素気流を通じることによって、雰囲気の窒素置換を行い、60℃まで昇温した。反応器の内部の温度が60℃になった時点で、硫酸第一鉄0.0001部、エチレンジアミン四酢酸二ナトリウム塩0.0003部及びロンガリット0.24部をイオン交換水10部に溶解させた水溶液を添加し、ラジカル重合を開始させた。アクリレート成分の重合により、液温は78℃まで上昇した。1時間この状態を維持し、アクリレート成分の重合を完結させて、ポリオルガノシロキサン(Ea)と(メタ)アクリル酸エステル系単量体単位と架橋剤および/またはグラフト交叉剤とを含有するポリ(メタ)アクリル酸エステルとからなる複合ゴム状重合体(E−2)の水性分散体を得た。水性分散体に分散している複合ゴム状重合体(E−2)の体積平均粒子径は0.04μmであった。
反応器内部の液温が60℃に低下した後、ロンガリット0.4部をイオン交換水10部に溶解した水溶液を添加した。次いで、アクリロニトリル11.1部、スチレン33.2部及びターシャリーブチルハイドロパーオキサイド0.2部の混合液を約1時間にわたって滴下し重合した。滴下終了後1時間保持した後、硫酸第一鉄0.0002部、エチレンジアミン四酢酸二ナトリウム塩0.0006部及びロンガリット0.25部をイオン交換水10部に溶解させた水溶液を添加した。次いで、アクリロニトリル7.4部、スチレン22.2部及びターシャリーブチルハイドロパーオキサイド0.1部の混合液を約40分間にわたって滴下し重合した。滴下終了後1時間保持した後、冷却して、複合ゴム状重合体(E−2)にアクリロニトリル−スチレン共重合体をグラフトさせたグラフト共重合体(F−2)の水性分散体を得た。次いで、酢酸カルシウムを5%の割合で溶解した水溶液150部を60℃に加熱し撹拌した。その酢酸カルシウム水溶液中にグラフト共重合体(F−2)の水性分散体100部を徐々に滴下して凝固させた。得られた凝固物を分離し、洗浄した後、乾燥させて、グラフト共重合体(F−2)の乾燥粉末を得た。
(Preparation of graft copolymer (F-2))
In a reactor equipped with a reagent injection container, a condenser tube, a jacket heater and a stirrer, 119.5 parts of an aqueous polyorganosiloxane (Ea) dispersion and 0.94 part of sodium polyoxyethylene alkylphenyl ether sulfate were charged. 203 parts of ion exchange water was added and mixed. Thereafter, a mixture consisting of 53.2 parts of n-butyl acrylate, 0.21 part of allyl methacrylate, 0.11 part of 1,3-butylene glycol dimethacrylate and 0.13 part of tertiary butyl hydroperoxide was added. The atmosphere was purged with nitrogen by passing a nitrogen stream through the reactor, and the temperature was raised to 60 ° C. When the temperature inside the reactor reached 60 ° C, 0.0001 part of ferrous sulfate, 0.0003 part of disodium ethylenediaminetetraacetic acid and 0.24 part of Rongalite were dissolved in 10 parts of ion-exchanged water. An aqueous solution was added to initiate radical polymerization. The liquid temperature rose to 78 ° C. by polymerization of the acrylate component. This state is maintained for 1 hour, polymerization of the acrylate component is completed, and poly (siloxane) containing polyorganosiloxane (Ea), a (meth) acrylate monomer unit, a crosslinking agent and / or a graft crossing agent is contained. An aqueous dispersion of a composite rubber-like polymer (E-2) composed of a (meth) acrylic ester was obtained. The composite rubber-like polymer (E-2) dispersed in the aqueous dispersion had a volume average particle size of 0.04 μm.
After the liquid temperature inside the reactor dropped to 60 ° C., an aqueous solution in which 0.4 part of Rongalite was dissolved in 10 parts of ion-exchanged water was added. Subsequently, 11.1 parts of acrylonitrile, 33.2 parts of styrene, and 0.2 part of tertiary butyl hydroperoxide were dropped and polymerized over about 1 hour. After holding for 1 hour after the completion of dropping, an aqueous solution in which 0.0002 parts of ferrous sulfate, 0.0006 parts of ethylenediaminetetraacetic acid disodium salt and 0.25 parts of Rongalite were dissolved in 10 parts of ion-exchanged water was added. Next, a mixture of 7.4 parts of acrylonitrile, 22.2 parts of styrene, and 0.1 part of tertiary butyl hydroperoxide was added dropwise over about 40 minutes for polymerization. After the completion of dropping, the mixture was kept for 1 hour and then cooled to obtain an aqueous dispersion of a graft copolymer (F-2) obtained by grafting an acrylonitrile-styrene copolymer onto a composite rubber-like polymer (E-2). . Next, 150 parts of an aqueous solution in which calcium acetate was dissolved at a rate of 5% was heated to 60 ° C. and stirred. 100 parts of an aqueous dispersion of the graft copolymer (F-2) was gradually dropped into the calcium acetate aqueous solution to be solidified. The obtained solidified product was separated, washed, and dried to obtain a dry powder of the graft copolymer (F-2).

(グラフト共重合体(F−3)の調製)
試薬注入容器、冷却管、ジャケット加熱器及び撹拌装置を備えた反応器内に、ポリオルガノシロキサン(Ea)水性分散体119.5部、ポリオキシエチレンアルキルフェニルエーテル硫酸ナトリウム0.9部を仕込み、イオン交換水203部を添加し、混合した。その後、n−ブチルアクリレート53.2部、アリルメタクリレート0.21部、1,3−ブチレングリコールジメタクリレート0.11部及びターシャリーブチルハイドロパーオキサイド0.13部からなる混合物を添加した。この反応器に窒素気流を通じることによって、雰囲気の窒素置換を行い、60℃まで昇温した。反応器の内部の温度が60℃になった時点で、硫酸第一鉄0.0001部、エチレンジアミン四酢酸二ナトリウム塩0.0003部及びロンガリット0.24部をイオン交換水10部に溶解させた水溶液を添加し、ラジカル重合を開始させた。アクリレート成分の重合により、液温は78℃まで上昇した。1時間この状態を維持し、アクリレート成分の重合を完結させて、ポリオルガノシロキサン(Ea) と( メタ) アクリル酸エステル系単量体単位と架橋剤および/ またはグラフト交叉剤とを含有するポリ(メタ)アクリル酸エステル とからなる複合ゴム状重合体(E−3)の水性分散体を得た。水性分散体に分散している複合ゴム状重合体(E−3)の体積平均粒子径は0.05μmであった。
反応器内部の液温が60℃に低下した後、ロンガリット0.4部をイオン交換水10部に溶解した水溶液を添加した。次いで、アクリロニトリル11.1部、スチレン33.2部及びターシャリーブチルハイドロパーオキサイド0.2部の混合液を約1時間にわたって滴下し重合した。滴下終了後1時間保持した後、硫酸第一鉄0.0002部、エチレンジアミン四酢酸二ナトリウム塩0.0006部及びロンガリット0.25部をイオン交換水10部に溶解させた水溶液を添加した。次いで、アクリロニトリル7.4部、スチレン22.2部及びターシャリーブチルハイドロパーオキサイド0.1部の混合液を約40分間にわたって滴下し重合した。滴下終了後1時間保持した後、冷却して、複合ゴム状重合体(E−3)にアクリロニトリル−スチレン共重合体をグラフトさせたグラフト共重合体(F−3)の水性分散体を得た。次いで、酢酸カルシウムを5%の割合で溶解した水溶液150部を60℃に加熱し撹拌した。その酢酸カルシウム水溶液中にグラフト共重合体(F−3)の水性分散体100部を徐々に滴下して凝固させた。得られた凝固物を分離し、洗浄した後、乾燥させて、グラフト共重合体(F−3)の乾燥粉末を得た。
(Preparation of graft copolymer (F-3))
In a reactor equipped with a reagent injection container, a condenser, a jacket heater and a stirrer, 119.5 parts of an aqueous dispersion of polyorganosiloxane (Ea) and 0.9 part of sodium polyoxyethylene alkylphenyl ether sulfate were charged. 203 parts of ion exchange water was added and mixed. Thereafter, a mixture consisting of 53.2 parts of n-butyl acrylate, 0.21 part of allyl methacrylate, 0.11 part of 1,3-butylene glycol dimethacrylate and 0.13 part of tertiary butyl hydroperoxide was added. The atmosphere was purged with nitrogen by passing a nitrogen stream through the reactor, and the temperature was raised to 60 ° C. When the temperature inside the reactor reached 60 ° C, 0.0001 part of ferrous sulfate, 0.0003 part of disodium ethylenediaminetetraacetic acid and 0.24 part of Rongalite were dissolved in 10 parts of ion-exchanged water. An aqueous solution was added to initiate radical polymerization. The liquid temperature rose to 78 ° C. by polymerization of the acrylate component. This state is maintained for 1 hour, polymerization of the acrylate component is completed, and poly (siloxane) containing polyorganosiloxane (Ea), (meth) acrylic acid ester monomer units, a crosslinking agent and / or a graft crossing agent is contained. An aqueous dispersion of a composite rubber-like polymer (E-3) comprising (meth) acrylic acid ester was obtained. The volume average particle diameter of the composite rubber-like polymer (E-3) dispersed in the aqueous dispersion was 0.05 μm.
After the liquid temperature inside the reactor dropped to 60 ° C., an aqueous solution in which 0.4 part of Rongalite was dissolved in 10 parts of ion-exchanged water was added. Subsequently, 11.1 parts of acrylonitrile, 33.2 parts of styrene, and 0.2 part of tertiary butyl hydroperoxide were dropped and polymerized over about 1 hour. After holding for 1 hour after the completion of dropping, an aqueous solution in which 0.0002 parts of ferrous sulfate, 0.0006 parts of ethylenediaminetetraacetic acid disodium salt and 0.25 parts of Rongalite were dissolved in 10 parts of ion-exchanged water was added. Next, a mixture of 7.4 parts of acrylonitrile, 22.2 parts of styrene, and 0.1 part of tertiary butyl hydroperoxide was added dropwise over about 40 minutes for polymerization. After holding for 1 hour after the completion of dropping, the mixture was cooled to obtain an aqueous dispersion of a graft copolymer (F-3) in which an acrylonitrile-styrene copolymer was grafted to the composite rubber-like polymer (E-3). . Next, 150 parts of an aqueous solution in which calcium acetate was dissolved at a rate of 5% was heated to 60 ° C. and stirred. 100 parts of an aqueous dispersion of the graft copolymer (F-3) was gradually dropped into the aqueous calcium acetate solution to be solidified. The obtained solidified product was separated, washed, and dried to obtain a dry powder of the graft copolymer (F-3).

(グラフト共重合体(F−4)の調製)
試薬注入容器、冷却管、ジャケット加熱器及び撹拌装置を備えた反応器内に、ポリオルガノシロキサン(Ea)水性分散体119.5部、ポリオキシエチレンアルキルフェニルエーテル硫酸ナトリウム0.51部を仕込み、イオン交換水203部を添加し、混合した。その後、n−ブチルアクリレート53.2部、アリルメタクリレート0.21部、1,3−ブチレングリコールジメタクリレート0.11部及びターシャリーブチルハイドロパーオキサイド0.13部からなる混合物を添加した。この反応器に窒素気流を通じることによって、雰囲気の窒素置換を行い、60℃まで昇温した。反応器の内部の温度が60℃になった時点で、硫酸第一鉄0.0001部、エチレンジアミン四酢酸二ナトリウム塩0.0003部及びロンガリット0.24部をイオン交換水10部に溶解させた水溶液を添加し、ラジカル重合を開始させた。アクリレート成分の重合により、液温は78℃まで上昇した。1時間この状態を維持し、アクリレート成分の重合を完結させて、ポリオルガノシロキサン(Ea)と(メタ)アクリル酸エステル系単量体単位と架橋剤および/またはグラフト交叉剤とを含有するポリ(メタ)アクリル酸エステルとからなる複合ゴム状重合体(E−4)の水性分散体を得た。水性分散体に分散している複合ゴム状重合体(E−4)の体積平均粒子径は0.18μmであった。
反応器内部の液温が60℃に低下した後、ロンガリット0.4部をイオン交換水10部に溶解した水溶液を添加した。次いで、アクリロニトリル11.1部、スチレン33.2部及びターシャリーブチルハイドロパーオキサイド0.2部の混合液を約1時間にわたって滴下し重合した。滴下終了後1時間保持した後、硫酸第一鉄0.0002部、エチレンジアミン四酢酸二ナトリウム塩0.0006部及びロンガリット0.25部をイオン交換水10部に溶解させた水溶液を添加した。次いで、アクリロニトリル7.4部、スチレン22.2部及びターシャリーブチルハイドロパーオキサイド0.1部の混合液を約40分間にわたって滴下し重合した。滴下終了後1時間保持した後、冷却して、複合ゴム状重合体(E−4)にアクリロニトリル−スチレン共重合体をグラフトさせたグラフト共重合体(F−4)の水性分散体を得た。次いで、酢酸カルシウムを5%の割合で溶解した水溶液150部を60℃に加熱し撹拌した。その酢酸カルシウム水溶液中にグラフト共重合体(F−4)の水性分散体100部を徐々に滴下して凝固させた。得られた凝固物を分離し、洗浄した後、乾燥させて、グラフト共重合体(F−4)の乾燥粉末を得た。
(Preparation of graft copolymer (F-4))
In a reactor equipped with a reagent injection container, a condenser, a jacket heater and a stirrer, 119.5 parts of an aqueous dispersion of polyorganosiloxane (Ea) and 0.51 part of sodium polyoxyethylene alkylphenyl ether sulfate were charged. 203 parts of ion exchange water was added and mixed. Thereafter, a mixture consisting of 53.2 parts of n-butyl acrylate, 0.21 part of allyl methacrylate, 0.11 part of 1,3-butylene glycol dimethacrylate and 0.13 part of tertiary butyl hydroperoxide was added. The atmosphere was purged with nitrogen by passing a nitrogen stream through the reactor, and the temperature was raised to 60 ° C. When the temperature inside the reactor reached 60 ° C, 0.0001 part of ferrous sulfate, 0.0003 part of disodium ethylenediaminetetraacetic acid and 0.24 part of Rongalite were dissolved in 10 parts of ion-exchanged water. An aqueous solution was added to initiate radical polymerization. The liquid temperature rose to 78 ° C. by polymerization of the acrylate component. This state is maintained for 1 hour, polymerization of the acrylate component is completed, and poly (siloxane) containing polyorganosiloxane (Ea), a (meth) acrylate monomer unit, a crosslinking agent and / or a graft crossing agent is contained. An aqueous dispersion of a composite rubber-like polymer (E-4) composed of (meth) acrylic acid ester was obtained. The volume average particle diameter of the composite rubber-like polymer (E-4) dispersed in the aqueous dispersion was 0.18 μm.
After the liquid temperature inside the reactor dropped to 60 ° C., an aqueous solution in which 0.4 part of Rongalite was dissolved in 10 parts of ion-exchanged water was added. Subsequently, 11.1 parts of acrylonitrile, 33.2 parts of styrene, and 0.2 part of tertiary butyl hydroperoxide were dropped and polymerized over about 1 hour. After holding for 1 hour after the completion of dropping, an aqueous solution in which 0.0002 parts of ferrous sulfate, 0.0006 parts of ethylenediaminetetraacetic acid disodium salt and 0.25 parts of Rongalite were dissolved in 10 parts of ion-exchanged water was added. Next, a mixture of 7.4 parts of acrylonitrile, 22.2 parts of styrene, and 0.1 part of tertiary butyl hydroperoxide was added dropwise over about 40 minutes for polymerization. After holding for 1 hour after the completion of dropping, the mixture was cooled to obtain an aqueous dispersion of a graft copolymer (F-4) obtained by grafting an acrylonitrile-styrene copolymer onto a composite rubber-like polymer (E-4). . Next, 150 parts of an aqueous solution in which calcium acetate was dissolved at a rate of 5% was heated to 60 ° C. and stirred. 100 parts of an aqueous dispersion of the graft copolymer (F-4) was gradually dropped into the calcium acetate aqueous solution to be solidified. The obtained solidified product was separated, washed, and dried to obtain a dry powder of the graft copolymer (F-4).

(グラフト共重合体(F−5)の調製)
試薬注入容器、冷却管、ジャケット加熱器及び撹拌装置を備えた反応器内に、ポリオルガノシロキサン(Ea)水性分散体119.5部、ポリオキシエチレンアルキルフェニルエーテル硫酸ナトリウム0.33部を仕込み、イオン交換水203部を添加し、混合した。その後、n−ブチルアクリレート53.2部、アリルメタクリレート0.21部、1,3−ブチレングリコールジメタクリレート0.11部及びターシャリーブチルハイドロパーオキサイド0.13部からなる混合物を添加した。この反応器に窒素気流を通じることによって、雰囲気の窒素置換を行い、60℃まで昇温した。反応器の内部の温度が60℃になった時点で、硫酸第一鉄0.0001部、エチレンジアミン四酢酸二ナトリウム塩0.0003部及びロンガリット0.24部をイオン交換水10部に溶解させた水溶液を添加し、ラジカル重合を開始させた。アクリレート成分の重合により、液温は78℃まで上昇した。1時間この状態を維持し、アクリレート成分の重合を完結させて、ポリオルガノシロキサン(Ea)と(メタ)アクリル酸エステル系単量体単位と架橋剤および/またはグラフト交叉剤とを含有するポリ(メタ)アクリル酸エステルとからなる複合ゴム状重合体(E−5)の水性分散体を得た。水性分散体に分散している複合ゴム状重合体(E−5)の体積平均粒子径は0.24μmであった。
反応器内部の液温が60℃に低下した後、ロンガリット0.4部をイオン交換水10部に溶解した水溶液を添加した。次いで、アクリロニトリル11.1部、スチレン33.2部及びターシャリーブチルハイドロパーオキサイド0.2部の混合液を約1時間にわたって滴下し重合した。滴下終了後1時間保持した後、硫酸第一鉄0.0002部、エチレンジアミン四酢酸二ナトリウム塩0.0006部及びロンガリット0.25部をイオン交換水10部に溶解させた水溶液を添加した。次いで、アクリロニトリル7.4部、スチレン22.2部及びターシャリーブチルハイドロパーオキサイド0.1部の混合液を約40分間にわたって滴下し重合した。滴下終了後1時間保持した後、冷却して、複合ゴム状重合体(E−5)にアクリロニトリル−スチレン共重合体をグラフトさせたグラフト共重合体(F−5)の水性分散体を得た。次いで、酢酸カルシウムを5%の割合で溶解した水溶液150部を60℃に加熱し撹拌した。その酢酸カルシウム水溶液中にグラフト共重合体(F−5)の水性分散体100部を徐々に滴下して凝固させた。得られた凝固物を分離し、洗浄した後、乾燥させて、グラフト重合体共(F−5)の乾燥粉末を得た。
(Preparation of graft copolymer (F-5))
In a reactor equipped with a reagent injection container, a condenser, a jacket heater and a stirrer, 119.5 parts of an aqueous polyorganosiloxane (Ea) dispersion and 0.33 part of sodium polyoxyethylene alkylphenyl ether sulfate were charged. 203 parts of ion exchange water was added and mixed. Thereafter, a mixture consisting of 53.2 parts of n-butyl acrylate, 0.21 part of allyl methacrylate, 0.11 part of 1,3-butylene glycol dimethacrylate and 0.13 part of tertiary butyl hydroperoxide was added. The atmosphere was purged with nitrogen by passing a nitrogen stream through the reactor, and the temperature was raised to 60 ° C. When the temperature inside the reactor reached 60 ° C, 0.0001 part of ferrous sulfate, 0.0003 part of disodium ethylenediaminetetraacetic acid and 0.24 part of Rongalite were dissolved in 10 parts of ion-exchanged water. An aqueous solution was added to initiate radical polymerization. The liquid temperature rose to 78 ° C. by polymerization of the acrylate component. This state is maintained for 1 hour, polymerization of the acrylate component is completed, and poly (siloxane) containing polyorganosiloxane (Ea), a (meth) acrylate monomer unit, a crosslinking agent and / or a graft crossing agent is contained. An aqueous dispersion of a composite rubber-like polymer (E-5) composed of (meth) acrylate was obtained. The volume average particle diameter of the composite rubber-like polymer (E-5) dispersed in the aqueous dispersion was 0.24 μm.
After the liquid temperature inside the reactor dropped to 60 ° C., an aqueous solution in which 0.4 part of Rongalite was dissolved in 10 parts of ion-exchanged water was added. Subsequently, 11.1 parts of acrylonitrile, 33.2 parts of styrene, and 0.2 part of tertiary butyl hydroperoxide were dropped and polymerized over about 1 hour. After holding for 1 hour after the completion of dropping, an aqueous solution in which 0.0002 parts of ferrous sulfate, 0.0006 parts of ethylenediaminetetraacetic acid disodium salt and 0.25 parts of Rongalite were dissolved in 10 parts of ion-exchanged water was added. Next, a mixture of 7.4 parts of acrylonitrile, 22.2 parts of styrene, and 0.1 part of tertiary butyl hydroperoxide was added dropwise over about 40 minutes for polymerization. After the completion of dropping, the mixture was kept for 1 hour and then cooled to obtain an aqueous dispersion of a graft copolymer (F-5) obtained by grafting an acrylonitrile-styrene copolymer onto a composite rubber-like polymer (E-5). . Next, 150 parts of an aqueous solution in which calcium acetate was dissolved at a rate of 5% was heated to 60 ° C. and stirred. 100 parts of an aqueous dispersion of the graft copolymer (F-5) was gradually dropped into the calcium acetate aqueous solution to be solidified. The obtained solidified product was separated, washed, and dried to obtain a dry powder of the graft polymer (F-5).

(グラフト共重合体(F−6)の調製)
撹拌機を備えた耐圧容器に脱イオン水150部、ブタジエンモノマー100部、硬化脂肪酸カリ石鹸3.0部、有機スルホン酸ソーダ0.3部、ターシャルドデシルメルカプタン0.2部、過硫酸カリウム0.3部、及び水酸化カリウム0.14部を仕込み、窒素雰囲気下で撹拌しながら温度を60℃に上げて重合を開始し、重合率65%のときに過硫酸カリウム0.1部を溶解した脱イオン水5部を上記耐圧容器に加えて重合温度を70℃に上げ、反応時間13時間、重合転化率95%で重合を完結し、平均粒子径0.10μm、固形分52.0%のゴム状重合体(E−6)のラテックスを得た。
試薬注入容器、冷却管、ジャケット加熱機および撹拌装置を備えた反応器内に、イオン交換水200部(ポリブタジエンラテックス中の水も含む)、不均化ロジン酸カリウム0.3部(固形分)、硫酸第一鉄七水塩0.01部、ピロリン酸ナトリウム0.2部、結晶ブドウ糖0.5部を仕込み、完全に溶解した後に、ゴム状重合体(E−6)のラテックス(固形分50部)を添加、混合した。
反応器内の内容物を撹拌しながら60℃まで昇温させ、スチレン39部とアクリロニトリル11部を2時間かけて連続的に滴下、供給してグラフト重合させた。その間、反応器内温を60℃に保つようにジャケット温度を制御した。滴下終了後70℃まで昇温させ、さらに1時間保ってグラフト重合反応を完結させた。冷却後、酸化防止剤(ジラウリルチオジプロピオネート)を添加し、グラフト共重合体(F−6)のラテックスを得た。
得られたグラフト共重合体(F−6)のラテックスを、その1倍量の2.5%硫酸水溶液(80℃)中に撹拌下で投入し、さらに90℃で5分間保持して凝固させてグラフト共重合体(F−6)のスラリーを得た。そして、そのスラリーの水洗と脱水を2度繰り返した後、一晩70℃で静置し、乾燥して乳白色粉末のグラフト共重合体(F−6)を得た。
(Preparation of graft copolymer (F-6))
In a pressure vessel equipped with a stirrer, 150 parts of deionized water, 100 parts of butadiene monomer, 3.0 parts of hardened fatty acid potassium soap, 0.3 part of sodium organic sulfonate, 0.2 part of tert-decyl mercaptan, 0 potassium persulfate .3 parts and 0.14 part of potassium hydroxide were added, the temperature was raised to 60 ° C. while stirring in a nitrogen atmosphere, and the polymerization was started. When the polymerization rate was 65%, 0.1 part of potassium persulfate was dissolved. 5 parts of the deionized water was added to the above pressure vessel, the polymerization temperature was raised to 70 ° C., the polymerization was completed at a reaction time of 13 hours and a polymerization conversion of 95%, an average particle size of 0.10 μm, and a solid content of 52.0%. A rubbery polymer (E-6) latex was obtained.
In a reactor equipped with a reagent injection container, a condenser, a jacket heater and a stirrer, 200 parts of ion-exchanged water (including water in polybutadiene latex), 0.3 part of disproportionated potassium rosinate (solid content) Then, 0.01 part of ferrous sulfate heptahydrate, 0.2 part of sodium pyrophosphate and 0.5 part of crystalline glucose were charged and completely dissolved, and then the latex of rubbery polymer (E-6) (solid content) 50 parts) was added and mixed.
While stirring the contents in the reactor, the temperature was raised to 60 ° C., and 39 parts of styrene and 11 parts of acrylonitrile were continuously added dropwise over 2 hours for graft polymerization. Meanwhile, the jacket temperature was controlled so as to keep the reactor internal temperature at 60 ° C. After completion of the dropwise addition, the temperature was raised to 70 ° C. and maintained for 1 hour to complete the graft polymerization reaction. After cooling, an antioxidant (dilauryl thiodipropionate) was added to obtain a latex of graft copolymer (F-6).
The obtained latex of the graft copolymer (F-6) was put into a 2.5% aqueous sulfuric acid solution (80 ° C.) of 1 volume with stirring, and further coagulated by holding at 90 ° C. for 5 minutes. Thus, a slurry of the graft copolymer (F-6) was obtained. The slurry was washed twice with water and dehydrated twice, then allowed to stand at 70 ° C. overnight and dried to obtain a milky white powder graft copolymer (F-6).

(グラフト共重合体(F−7)の調製)
アルケニルコハク酸ジカリウム0.6部、イオン交換水175部、アクリル酸n−ブチル50部、メタクリル酸アリル0.16部、1,3−ブチレングリコールジメタクリレート0.08部、およびt−ブチルヒドロペルオキシド0.1部の混合物を反応器に投入した。反応器に窒素気流を通じることによって、反応器内を窒素置換し、60℃まで昇温した。内温が50℃となった時点で、硫酸第一鉄0.00015部、エチレンジアミン四酢酸二ナトリウム塩0.00045部、ロンガリット0.24部、およびイオン交換水5部からなる水溶液を添加して重合を開始させ、内温を75℃に上昇させた。さらにこの状態を1時間維持し、平均粒子径0.11μmのゴム状重合体(E−7)を得た。
反応器の内温を75℃に保ったまま、ゴム状重合体(E−7)50部(固形分として)に対して、ロンガリット0.15部、アルケニルコハク酸ジカリウム0.65部、およびイオン交換水10部からなる水溶液を添加し、ついで、アクリロニトリル6.3部、スチレン18.7部、およびt−ブチルヒドロペルオキシド0.11部からなる混合液を1時間にわたって滴下し、グラフト重合させた。滴下終了から5分後に、硫酸第一鉄0.001部、エチレンジアミン四酢酸二ナトリウム塩0.003部、ロンガリット0.15部、およびイオン交換水5部からなる水溶液を添加し、ついで、アクリロニトリル11部、スチレン39部、t−ブチルヒドロペルオキシド0.19部、およびn−オクチルメルカプタン0.014部からなる混合液を1時間にわたって滴下しグラフト重合させた。滴下終了後、内温を75℃に10分間保持した後、冷却し、内温が60℃となった時点で、酸化防止剤(吉富製薬工業社製、アンテージW500)0.2部およびアルケニルコハク酸ジカリウム0.2部をイオン交換水5部に溶解した水溶液を添加した。ついで、反応生成物の水性分散体を硫酸水溶液で凝固、水洗した後、乾燥してグラフト共重合体(F−7)を得た。
(Preparation of graft copolymer (F-7))
0.6 parts of dipotassium alkenyl succinate, 175 parts of ion exchange water, 50 parts of n-butyl acrylate, 0.16 part of allyl methacrylate, 0.08 part of 1,3-butylene glycol dimethacrylate, and t-butyl hydroperoxide 0.1 part of the mixture was charged to the reactor. By passing a nitrogen stream through the reactor, the inside of the reactor was purged with nitrogen, and the temperature was raised to 60 ° C. When the internal temperature reached 50 ° C., an aqueous solution consisting of 0.00015 part of ferrous sulfate, 0.00045 part of ethylenediaminetetraacetic acid disodium salt, 0.24 part of Rongalite, and 5 parts of ion-exchanged water was added. Polymerization was started and the internal temperature was raised to 75 ° C. Furthermore, this state was maintained for 1 hour to obtain a rubber-like polymer (E-7) having an average particle size of 0.11 μm.
While maintaining the internal temperature of the reactor at 75 ° C., 0.15 part of Rongalite, 0.65 part of dipotassium alkenyl succinate, and ions with respect to 50 parts (as a solid content) of the rubber-like polymer (E-7) An aqueous solution consisting of 10 parts of exchange water was added, and then a mixed liquid consisting of 6.3 parts of acrylonitrile, 18.7 parts of styrene, and 0.11 part of t-butyl hydroperoxide was added dropwise over 1 hour for graft polymerization. . Five minutes after the completion of dropping, an aqueous solution comprising 0.001 part of ferrous sulfate, 0.003 part of ethylenediaminetetraacetic acid disodium salt, 0.15 part of Rongalite, and 5 parts of ion-exchanged water was added, and then acrylonitrile 11 A mixture consisting of 39 parts of styrene, 39 parts of styrene, 0.19 part of t-butyl hydroperoxide, and 0.014 part of n-octyl mercaptan was added dropwise over 1 hour for graft polymerization. After completion of the dropwise addition, the internal temperature was kept at 75 ° C. for 10 minutes and then cooled. When the internal temperature reached 60 ° C., 0.2 parts of antioxidant (Yantomi Pharmaceutical Co., Ltd., Antage W500) and alkenyl succinic acid were added. An aqueous solution in which 0.2 part of dipotassium acid was dissolved in 5 parts of ion-exchanged water was added. Subsequently, the aqueous dispersion of the reaction product was coagulated with an aqueous sulfuric acid solution, washed with water, and dried to obtain a graft copolymer (F-7).

グラフト共重合体(F−1)〜(F−7)の調製に用いたゴム状重合体(E)およびグラフト共重合体(F)中のゴム状重合体(E)の平均粒子径を表10に示す。   The average particle diameter of the rubber-like polymer (E) used in the preparation of the graft copolymers (F-1) to (F-7) and the rubber-like polymer (E) in the graft copolymer (F) is shown. 10 shows.

Figure 0006291702
Figure 0006291702

<メタクリル酸エステル樹脂(G)>
(メタクリル酸エステル樹脂(G−1)の調製)
撹拌機付きステンレス重合槽にイオン交換水150部、メタクリル酸メチル99部、アクリル酸メチル1部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、カルシウムヒドロオキシアパタイト0.47部、アルケニルコハク酸カリウム0.003部を仕込んだ。重合槽の内温を75℃にして3時間反応させ、90℃に昇温し1時間反応させた。内容物を抜き出し、遠心脱水機で洗浄し、乾燥させて粉状のメタクリル酸エステル樹脂(G−1)を得た。単量体の使用量を表11に示す。
<Methacrylate ester resin (G)>
(Preparation of methacrylate resin (G-1))
In a stainless polymerization tank equipped with a stirrer, 150 parts of ion exchange water, 99 parts of methyl methacrylate, 1 part of methyl acrylate, 0.2 part of 2,2′-azobis (isobutyronitrile), 0.25 part of n-octyl mercaptan , 0.47 part of calcium hydroxyapatite and 0.003 part of potassium alkenyl succinate were charged. The internal temperature of the polymerization tank was set to 75 ° C. for 3 hours, and the temperature was raised to 90 ° C. for 1 hour. The contents were extracted, washed with a centrifugal dehydrator, and dried to obtain a powdered methacrylate resin (G-1). The amount of monomer used is shown in Table 11.

(メタクリル酸エステル樹脂(G−2)の調製)
撹拌機付きステンレス重合槽にイオン交換水150部、メタクリル酸メチル82部、N−フェニルマレイミド12部、スチレン6部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、ポリビニルアルコール0.7部を仕込んだ。重合槽の内温を75℃にして3時間反応させ、90℃まで昇温し1時間反応させた。内容物を抜き出し、遠心脱水機で洗浄し、乾燥させて粉状のメタクリル酸エステル樹脂(G−2)を得た。単量体の使用量を表11に示す。
(Preparation of methacrylate ester resin (G-2))
In a stainless polymerization tank equipped with a stirrer, 150 parts of ion exchange water, 82 parts of methyl methacrylate, 12 parts of N-phenylmaleimide, 6 parts of styrene, 0.2 part of 2,2′-azobis (isobutyronitrile), n-octyl Mercaptan (0.25 part) and polyvinyl alcohol (0.7 part) were charged. The internal temperature of the polymerization tank was set at 75 ° C. for 3 hours, and the temperature was raised to 90 ° C. for 1 hour. The contents were extracted, washed with a centrifugal dehydrator, and dried to obtain a powdered methacrylate resin (G-2). The amount of monomer used is shown in Table 11.

(シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G−3)の調製)
撹拌機付きステンレス重合槽に、MEK−ST(日産化学工業株式会社製オルガノシリカゾル、分散媒:メチルエチルケトン(MEK)、平均粒子径16nm)のMEKを留去することで得られたシリカ粒子(H)20部をメタクリル酸メチル79.2部、アクリル酸メチル0.8部からなる溶液に分散させた分散液、イオン交換水150部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、カルシウムヒドロオキシアパタイト0.47部、アルケニルコハク酸カリウム0.003部を仕込んだ。重合槽の内温を75℃にして3時間反応させ、90℃に昇温し1時間反応させた。内容物を抜き出し、遠心脱水機で洗浄し、乾燥させて粉状のメタクリル酸エステル樹脂(G−3)を得た。単量体およびシリカ粒子の使用量を表11に示す。
(Preparation of methacrylate resin (G-3) in which silica particles (H) are dispersed)
Silica particles (H) obtained by distilling off MEK-ST (organosilica sol manufactured by Nissan Chemical Industries, Ltd., dispersion medium: methyl ethyl ketone (MEK), average particle size 16 nm) in a stainless polymerization tank equipped with a stirrer 20 parts dispersed in a solution consisting of 79.2 parts methyl methacrylate and 0.8 parts methyl acrylate, 150 parts ion-exchanged water, 0.2 part 2,2′-azobis (isobutyronitrile) , 0.25 part of n-octyl mercaptan, 0.47 part of calcium hydroxyapatite and 0.003 part of potassium alkenyl succinate were charged. The internal temperature of the polymerization tank was set to 75 ° C. for 3 hours, and the temperature was raised to 90 ° C. for 1 hour. The contents were extracted, washed with a centrifugal dehydrator, and dried to obtain a powdery methacrylic ester resin (G-3). Table 11 shows the amounts of monomer and silica particles used.

(シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G−4)の調製)
撹拌機付きステンレス重合槽に、MEK−ST(日産化学工業株式会社製オルガノシリカゾル、分散媒:MEK、平均粒子径16nm)のMEKを留去することで得られたシリカ粒子(H)20部をメタクリル酸メチル65.6部、N−フェニルマレイミド9.6部、スチレン4.8部からなる溶液に分散させた分散液、イオン交換水150部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、カルシウムヒドロオキシアパタイト0.47部、アルケニルコハク酸カリウム0.003部を仕込んだ。重合槽の内温を75℃にして3時間反応させ、90℃に昇温し1時間反応させた。内容物を抜き出し、遠心脱水機で洗浄し、乾燥させて粉状のメタクリル酸エステル樹脂(G−4)を得た。単量体およびシリカ粒子の使用量を表11に示す。
(Preparation of methacrylate resin (G-4) in which silica particles (H) are dispersed)
In a stainless polymerization tank equipped with a stirrer, 20 parts of silica particles (H) obtained by distilling off MEK of MEK-ST (organosilica sol manufactured by Nissan Chemical Industries, Ltd., dispersion medium: MEK, average particle diameter 16 nm) Dispersion dispersed in a solution consisting of 65.6 parts of methyl methacrylate, 9.6 parts of N-phenylmaleimide and 4.8 parts of styrene, 150 parts of ion-exchanged water, 2,2′-azobis (isobutyronitrile) 0.2 part, 0.25 part of n-octyl mercaptan, 0.47 part of calcium hydroxyapatite and 0.003 part of potassium alkenyl succinate were charged. The internal temperature of the polymerization tank was set to 75 ° C. for 3 hours, and the temperature was raised to 90 ° C. for 1 hour. The contents were extracted, washed with a centrifugal dehydrator, and dried to obtain a powdered methacrylate resin (G-4). Table 11 shows the amounts of monomer and silica particles used.

Figure 0006291702
Figure 0006291702

<スチレン系共重合体(I)>
(スチレン系共重合体(I−1)の調製)
窒素置換した撹拌機付きステンレス重合槽に、イオン交換水120部、ポリビニルアルコール0.1部、2,2’−アゾビス(イソブチロニトリル)0.3部、アクリロニトリル25部、スチレン75部、t−ドデシルメルカプタン0.35部を仕込み、開始温度60℃として5時間反応させた。120℃に昇温し、4時間反応させた。内容物を取り出し、スチレン系共重合体(I−1)を得た。単量体の使用量を表12に示す。
<Styrene copolymer (I)>
(Preparation of styrene copolymer (I-1))
In a stainless steel polymerization tank equipped with a stirrer substituted with nitrogen, 120 parts of ion exchange water, 0.1 part of polyvinyl alcohol, 0.3 part of 2,2′-azobis (isobutyronitrile), 25 parts of acrylonitrile, 75 parts of styrene, t -0.35 part of dodecyl mercaptan was charged and reacted at an initial temperature of 60 ° C for 5 hours. The temperature was raised to 120 ° C. and reacted for 4 hours. The contents were taken out to obtain a styrene copolymer (I-1). The amount of monomer used is shown in Table 12.

(スチレン系共重合体(I−2)の調製)
撹拌機付きステンレス重合槽に、イオン交換水150部、メタクリル酸メチル10部、アクリロニトリル22部、スチレン68部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、カルシウムヒドロオキシアパタイト0.47部、アルケニルコハク酸カリウム0.003部を仕込み、内温を75℃まで昇温し、3時間反応させた。90℃まで昇温し、60分間保持することで反応を完結させた。内容物を取り出し、遠心脱水機での洗浄、脱水を繰り返し、乾燥させてスチレン系共重合体(I−2)を得た。単量体の使用量を表12に示す。
(Preparation of styrene copolymer (I-2))
In a stainless polymerization tank equipped with a stirrer, 150 parts of ion exchange water, 10 parts of methyl methacrylate, 22 parts of acrylonitrile, 68 parts of styrene, 0.2 part of 2,2′-azobis (isobutyronitrile), n-octyl mercaptan 0 .25 parts, calcium hydroxyapatite 0.47 part, and potassium alkenyl succinate 0.003 part were charged, the internal temperature was raised to 75 ° C., and the reaction was performed for 3 hours. The reaction was completed by raising the temperature to 90 ° C. and holding for 60 minutes. The contents were taken out, repeatedly washed with a centrifugal dehydrator and dehydrated, and dried to obtain a styrene copolymer (I-2). The amount of monomer used is shown in Table 12.

(スチレン系共重合体(I−3)の調製)
撹拌機付きステンレス重合槽に、イオン交換水150部、N−フェニルマレイミド30部、アクリロニトリル15部、スチレン55部、2,2’−アゾビス(イソブチロニトリル)0.2部、n−オクチルメルカプタン0.25部、カルシウムヒドロオキシアパタイト0.47部、アルケニルコハク酸カリウム0.003部を仕込み、内温を75℃まで昇温し、3時間反応させた。90℃まで昇温し、60分間保持することで反応を完結させた。内容物を取り出し、遠心脱水機での洗浄、脱水を繰り返し、乾燥させてスチレン系共重合体(I−3)を得た。単量体の使用量を表12に示す。
(Preparation of styrene copolymer (I-3))
In a stainless polymerization tank equipped with a stirrer, 150 parts of ion exchange water, 30 parts of N-phenylmaleimide, 15 parts of acrylonitrile, 55 parts of styrene, 0.2 part of 2,2′-azobis (isobutyronitrile), n-octyl mercaptan 0.25 part, 0.47 part of calcium hydroxyapatite and 0.003 part of potassium alkenyl succinate were charged, the internal temperature was raised to 75 ° C., and the reaction was performed for 3 hours. The reaction was completed by raising the temperature to 90 ° C. and holding for 60 minutes. The contents were taken out, repeatedly washed with a centrifugal dehydrator, dehydrated, and dried to obtain a styrene copolymer (I-3). The amount of monomer used is shown in Table 12.

Figure 0006291702
Figure 0006291702

[実施例1]
グラフト共重合体(D−2)10部、グラフト共重合体(F−1)14部、メタクリル酸エステル樹脂(G−2)36部、シリカ粒子(H)が分散したメタクリル酸エステル樹脂(G−4)50部(シリカ粒子(H)10部を含む。)を混合し、30mmφの真空ベント付き2軸押出機(池貝社製、「PCM30」)で240℃、93.325kPa真空にて溶融混練し、熱可塑性樹脂組成物を調製した。熱可塑性樹脂組成物のMVRを表13に示す。
熱可塑性樹脂組成物をペレット化し、各種成形品を成形し、耐衝撃性、耐寒衝撃性、発色性、耐引っ掻き傷性、耐擦り傷性、耐熱性、潤滑性(きしみ音)を評価した。結果を表13に示す。
[Example 1]
Graft copolymer (D-2) 10 parts, Graft copolymer (F-1) 14 parts, Methacrylate resin (G-2) 36 parts, Methacrylate resin (G) dispersed with silica particles (H) -4) 50 parts (including 10 parts of silica particles (H)) were mixed and melted at 240 ° C. and 93.325 kPa vacuum in a 30 mmφ twin-screw extruder with a vacuum vent (Ikegai Co., Ltd., “PCM30”). The mixture was kneaded to prepare a thermoplastic resin composition. Table 13 shows the MVR of the thermoplastic resin composition.
The thermoplastic resin composition was pelletized and various molded articles were molded, and the impact resistance, cold impact resistance, color development, scratch resistance, scratch resistance, heat resistance and lubricity (squeak noise) were evaluated. The results are shown in Table 13.

[実施例2〜45]
表13〜18(表13〜18中のシリカ粒子(H)(部)は、配合したメタクリル酸エステル樹脂(G−3)〜(G−4)中に含まれるシリカ粒子(H)の量を示す。)に示す配合処方に変更した以外は、実施例1と同様にして熱可塑性樹脂組成物を調製し、MVRを測定した。
熱可塑性樹脂組成物をペレット化し、各種成形品を成形し、耐衝撃性、耐寒衝撃性、発色性、耐引っ掻き傷性、耐擦り傷性、耐熱性、潤滑性(きしみ音)を評価した。結果を表13〜18に示す。
[Examples 2-45]
Tables 13 to 18 (silica particles (H) (parts) in Tables 13 to 18 indicate the amount of silica particles (H) contained in the blended methacrylate resins (G-3) to (G-4). A thermoplastic resin composition was prepared and MVR was measured in the same manner as in Example 1 except that the formulation was changed to the formulation shown in FIG.
The thermoplastic resin composition was pelletized and various molded articles were molded, and the impact resistance, cold impact resistance, color development, scratch resistance, scratch resistance, heat resistance and lubricity (squeak noise) were evaluated. The results are shown in Tables 13-18.

[比較例1〜14]
表19〜20(表19〜20中のシリカ粒子(H)(部)は、配合したメタクリル酸エステル樹脂(G−3)〜(G−4)中に含まれるシリカ粒子(H)の量を示す。)に示す配合処方に変更した以外は、実施例1と同様にして熱可塑性樹脂組成物を調製し、MVRを測定した。
熱可塑性樹脂組成物をペレット化し、各種成形品を成形し、耐衝撃性、耐寒衝撃性、発色性、耐引っ掻き傷性、耐擦り傷性、耐熱性、潤滑性(きしみ音)を評価した。結果を表19〜20に示す。
[Comparative Examples 1-14]
Tables 19 to 20 (silica particles (H) (parts) in Tables 19 to 20 indicate the amount of silica particles (H) contained in the blended methacrylate resins (G-3) to (G-4). A thermoplastic resin composition was prepared and MVR was measured in the same manner as in Example 1 except that the formulation was changed to the formulation shown in FIG.
The thermoplastic resin composition was pelletized and various molded articles were molded, and the impact resistance, cold impact resistance, color development, scratch resistance, scratch resistance, heat resistance and lubricity (squeak noise) were evaluated. The results are shown in Tables 19-20.

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

Figure 0006291702
Figure 0006291702

実施例1〜45の熱可塑性樹脂組成物は流動性に優れていた。また、実施例1〜45で得られた成形品は、耐引っ掻き傷性、耐擦り傷性、耐衝撃性、耐寒衝撃性、発色性、潤滑性(きしみ音)、耐熱性、耐候性が優れていた。
一方、比較例1〜14で得られた成形品は、耐引っ掻き傷性、耐擦り傷性、耐衝撃性、耐寒衝撃性、発色性、潤滑性(きしみ音)のいずれか1以上の特性が不充分であった。
The thermoplastic resin compositions of Examples 1 to 45 were excellent in fluidity. In addition, the molded products obtained in Examples 1 to 45 are excellent in scratch resistance, scratch resistance, impact resistance, cold impact resistance, color development, lubricity (squeak noise), heat resistance, and weather resistance. It was.
On the other hand, the molded products obtained in Comparative Examples 1 to 14 have one or more characteristics of scratch resistance, scratch resistance, impact resistance, cold impact resistance, color development, and lubricity (squeak noise). It was enough.

したがって、本発明の熱可塑性樹脂組成物は、流動性が優れており、本発明の熱可塑性樹脂組成物を用いると、耐傷付き性、耐衝撃性、耐寒衝撃性、発色性、潤滑性に優れた成形品が得られ、車輌内外装部品、事務機器、家電、建材等の用途に適用できることがわかる。   Therefore, the thermoplastic resin composition of the present invention is excellent in fluidity, and when the thermoplastic resin composition of the present invention is used, it is excellent in scratch resistance, impact resistance, cold shock resistance, color development, and lubricity. It can be seen that the molded product can be applied to applications such as vehicle interior / exterior parts, office equipment, home appliances, and building materials.

本発明の熱可塑性樹脂組成物を用いた成形品は、車輌内外装部品、事務機器、家電、建材等として有用である。   A molded article using the thermoplastic resin composition of the present invention is useful as a vehicle interior / exterior part, office equipment, home appliance, building material and the like.

10 治具
11 先端部
12 積層シート
13 成形品(Ma2)
21 試験片
21a リブ構造
22 試験片
10 Jig 11 Tip 12 Laminated Sheet 13 Molded Product (Ma2)
21 Test piece 21a Rib structure 22 Test piece

Claims (4)

質量平均分子量(Mw)が17×10〜35×10であり、分子量分布(Mw/Mn)が1〜3であるエチレン・α−オレフィン共重合体(A)または該エチレン・α−オレフィン共重合体(A)を架橋処理した架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合して得られたグラフト共重合体(D)と、
ゴム状重合体(E)の存在下に、ビニル系単量体成分(m2)を重合して得られたグラフト共重合体(F)と、
メタクリル酸エステルを含むビニル系単量体成分(m3)を重合して得られたメタクリル酸エステル樹脂(G)と、
シリカ粒子(H)と、を含み、
前記グラフト重合体(D)に含まれるエチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の平均粒子径が、0.20μm〜0.60μmであり、
前記グラフト共重合体(F)に含まれるゴム状重合体(E)の平均粒子径が、0.05μm〜0.18μmであり、
前記エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)と前記ゴム状重合体(E)との合計(100質量%)のうち、エチレン・α−オレフィン共重合体(A)または架橋エチレン・α−オレフィン共重合体(C)の割合が、15〜85質量%であり、ゴム状重合体(E)の割合が、85〜15質量%である、熱可塑性樹脂組成物。
The ethylene / α-olefin copolymer (A) or the ethylene / α-olefin having a mass average molecular weight (Mw) of 17 × 10 4 to 35 × 10 4 and a molecular weight distribution (Mw / Mn) of 1 to 3 Graft copolymer (D) obtained by polymerizing vinyl monomer component (m1) in the presence of crosslinked ethylene / α-olefin copolymer (C) obtained by crosslinking copolymer (A) When,
A graft copolymer (F) obtained by polymerizing the vinyl monomer component (m2) in the presence of the rubber-like polymer (E);
A methacrylate ester resin (G) obtained by polymerizing a vinyl-based monomer component (m3) containing a methacrylate ester;
Silica particles (H),
The average particle diameter of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) contained in the graft polymer (D) is 0.20 μm to 0.60 μm,
The rubbery polymer (E) contained in the graft copolymer (F) has an average particle size of 0.05 μm to 0.18 μm,
Of the total (100% by mass) of the ethylene / α-olefin copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) and the rubbery polymer (E), ethylene / α-olefin The ratio of the copolymer (A) or the crosslinked ethylene / α-olefin copolymer (C) is 15 to 85% by mass, and the ratio of the rubbery polymer (E) is 85 to 15% by mass. Thermoplastic resin composition.
前記ゴム状重合体(E)が、シリコーン系−アクリル系複合ゴム状重合体である、請求項1に記載の熱可塑性樹脂組成物。The thermoplastic resin composition according to claim 1, wherein the rubber-like polymer (E) is a silicone-acrylic composite rubber-like polymer. 前記グラフト共重合体(D)が、前記架橋エチレン・α−オレフィン共重合体(C)の存在下に、ビニル系単量体成分(m1)を重合して得られたものである、請求項1または2に記載の熱可塑性樹脂組成物。 The graft copolymer (D) is obtained by polymerizing a vinyl monomer component (m1) in the presence of the crosslinked ethylene / α-olefin copolymer (C). The thermoplastic resin composition according to 1 or 2 . 請求項1〜3のいずれか一項に記載の熱可塑性樹脂組成物を用いた成形品。 The molded article using the thermoplastic resin composition as described in any one of Claims 1-3.
JP2014084810A 2014-04-16 2014-04-16 Thermoplastic resin composition and molded article thereof Active JP6291702B2 (en)