JP5552969B2 - Prepreg, substrate and semiconductor device - Google Patents

Prepreg, substrate and semiconductor device Download PDF

Info

Publication number
JP5552969B2
JP5552969B2 JP2010194260A JP2010194260A JP5552969B2 JP 5552969 B2 JP5552969 B2 JP 5552969B2 JP 2010194260 A JP2010194260 A JP 2010194260A JP 2010194260 A JP2010194260 A JP 2010194260A JP 5552969 B2 JP5552969 B2 JP 5552969B2
Authority
JP
Japan
Prior art keywords
resin
resin layer
prepreg
substrate
fiber base
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2010194260A
Other languages
Japanese (ja)
Other versions
JP2012051989A (en
Inventor
猛 八月朔日
恭史 瀧本
晴行 秦野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Bakelite Co Ltd
Original Assignee
Sumitomo Bakelite Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Bakelite Co Ltd filed Critical Sumitomo Bakelite Co Ltd
Priority to JP2010194260A priority Critical patent/JP5552969B2/en
Publication of JP2012051989A publication Critical patent/JP2012051989A/en
Application granted granted Critical
Publication of JP5552969B2 publication Critical patent/JP5552969B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、プリプレグ、基板および半導体装置に関する。   The present invention relates to a prepreg, a substrate, and a semiconductor device.

近年、電子部品・電子機器等を小型化・薄膜化すべく、これに用いられる回路基板等を小型化・薄膜化することが要求されている。この要求に答えるために、多層構造の回路基板を用い、その各層を薄くすることが行なわれている。   In recent years, in order to reduce the size and thickness of electronic components and electronic devices, it has been required to reduce the size and thickness of circuit boards used therefor. In order to meet this requirement, a circuit board having a multilayer structure is used and each layer is thinned.

多層構造の回路基板は、例えば2枚のプリプレグ(第1のプリプレグおよび第2のプリプレグ)を用いて製造される。一般に、このような構成の回路基板を薄くするためには、第1のプリプレグの一方の面に配線部を形成し、当該配線部を、この第1のプリプレグに積層される第2のプリプレグの他方の面に埋設することが行われる。   A circuit board having a multilayer structure is manufactured using, for example, two prepregs (a first prepreg and a second prepreg). In general, in order to thin the circuit board having such a configuration, a wiring portion is formed on one surface of the first prepreg, and the wiring portion is laminated on the first prepreg. Embedding on the other side is performed.

この場合、第1のプリプレグの一方の面側には、配線部を形成するための高い密着性が、第2のプリプレグの他方の面側には、配線部を埋め込むための高い埋め込み性が要求される。かかる特性を有するプリプレグとして、例えば、特許文献1には、繊維基材の両側に、異なる樹脂組成物で構成される2つの樹脂層を形成したプリプレグが開示されている。   In this case, high adhesion for forming the wiring portion is required on one surface side of the first prepreg, and high embedding property for embedding the wiring portion is required on the other surface side of the second prepreg. Is done. As a prepreg having such characteristics, for example, Patent Document 1 discloses a prepreg in which two resin layers made of different resin compositions are formed on both sides of a fiber base material.

そして、現状、かかるプリプレグにおいて、更なる機械的強度の向上、耐久性の向上等を目的として改良が行われている。   At present, such prepregs are improved for the purpose of further improving mechanical strength and durability.

国際公開第2007/063960号パンフレットInternational Publication No. 2007/063960 Pamphlet

本発明の目的は、プリプレグの両面に異なる用途、機能、性能または特性等を付与することができ、かつ、優れた機械的強度や耐久性を有するプリプレグ、このプリプレグを備える基板、およびかかる基板を用いて製造される半導体装置を提供することにある。   An object of the present invention is to provide a prepreg that can impart different uses, functions, performances, characteristics, etc. to both sides of the prepreg, and has excellent mechanical strength and durability, a substrate including the prepreg, and such a substrate. An object of the present invention is to provide a semiconductor device manufactured using the same.

このような目的は、下記(1)〜(9)の本発明により達成される。
(1) 平板状の繊維基材と、
前記繊維基材の一方の面側に位置し、第1の樹脂組成物で構成された第1の樹脂層と、
前記繊維基材の他方の面側に位置し、前記第1の樹脂組成物と異なる組成の第2の樹脂組成物で構成された第2の樹脂層とを備え、
前記第1の樹脂層は、前記繊維基材の厚さ方向の一部に前記第1の樹脂組成物が含浸した第1の含浸部を有し、
前記第2の樹脂層は、前記第1の樹脂層よりも可撓性が高いものであり、前記繊維基材の前記第1の樹脂組成物が含浸されていない残りの部分に前記第2の樹脂組成物が含浸した第2の含浸部を有し、
前記繊維基材内において、前記第1の含浸部と前記第2の含浸部とが接触しており、
前記第1の含浸部の平均厚さをt a1 [μm]とし、前記第2の含浸部の平均厚さをt b1 [μm]としたとき、t a1 >t b1 なる関係を満足することを特徴とするプリプレグ。
Such an object is achieved by the present inventions (1) to (9) below.
(1) a flat fiber substrate;
A first resin layer located on one side of the fiber substrate and composed of a first resin composition;
A second resin layer that is located on the other surface side of the fiber base material and is composed of a second resin composition having a composition different from that of the first resin composition;
The first resin layer has a first impregnation portion impregnated with the first resin composition in a part of the fiber base in the thickness direction;
The second resin layer is more flexible than the first resin layer, and the second resin layer is not impregnated with the first resin composition , and the second resin layer is not impregnated with the second resin layer. A second impregnation portion impregnated with the resin composition;
In the fiber substrate, the first impregnation part and the second impregnation part are in contact with each other,
When the average thickness of the first impregnated portion is t a1 [μm] and the average thickness of the second impregnated portion is t b1 [μm], the relationship t a1 > t b1 is satisfied. Characteristic prepreg.

(2) 前記第1の含浸部と前記第2の含浸部との界面は、凹凸をなす上記(1)に記載のプリプレグ。   (2) The prepreg according to (1) above, wherein an interface between the first impregnation part and the second impregnation part is uneven.

(3) 前記第2の樹脂層は、前記第1の樹脂層よりも可撓性が高いものであり、
前記第1の樹脂層の前記第1の含浸部を除く部分の平均厚さをta2[μm]とし、前記第2の樹脂層の前記第2の含浸部を除く部分の平均厚さをtb2[μm]としたとき、1.2×ta2<tb2なる関係を満足する上記(1)または(2)に記載のプリプレグ。
(3) The second resin layer is higher in flexibility than the first resin layer,
The average thickness of the portion of the first resin layer excluding the first impregnation portion is t a2 [μm], and the average thickness of the portion of the second resin layer excluding the second impregnation portion is t The prepreg according to the above (1) or (2) , which satisfies a relationship of 1.2 × t a2 <t b2 when b2 [μm].

(4) 前記第1の樹脂組成物および前記第2の樹脂組成物は、それぞれ、硬化性樹脂を含み、該硬化性樹脂の種類、含有量、分子量のうちの少なくとも1つが異なるものである上記(1)ないし(3)のいずれかに記載のプリプレグ。 (4) the first resin composition and the second resin composition, respectively, comprising a curable resin, the kind of the curable resin, the content, at least one of the molecular weight but different from the (1) thru | or the prepreg in any one of (3) .

(5) 前記繊維基材は、ガラス繊維基材である上記(1)ないし(4)のいずれかに記載のプリプレグ。 (5) the fiber base material, prepreg according to any one of Ru (1) to a glass fiber substrate der (4).

(6) 上記(1)ないし(5)のいずれかに記載のプリプレグを複数積層してなる積層体を備えることを特徴とする基板。 (6) A substrate comprising a laminate formed by laminating a plurality of the prepregs according to any one of (1) to (5 ) above .

(7) 隣接する前記プリプレグの間に繊維基材をさらに備える上記(6)に記載の基板。 (7) The substrate according to (6) , further including a fiber base material between the adjacent prepregs.

(8) 前記積層体の少なくとも一方の面に金属層をさらに備える上記(6)または(7)に記載の基板。 (8) The substrate according to (6) or (7) , further including a metal layer on at least one surface of the laminate.

(9) 上記(6)ないし(8)のいずれかに記載の基板と、
前記基板に搭載された半導体素子とを備えることを特徴とする半導体装置。
(9) The substrate according to any one of (6) to (8 ) above ,
A semiconductor device comprising: a semiconductor element mounted on the substrate.

本発明によれば、第1の樹脂層を構成する第1の樹脂組成物と第2の樹脂層を構成する第2の樹脂組成物とが互いに組成が異なるもの同士であるため、プリプレグの両面には、それぞれ、異なる用途、機能、性能または特性等を有する第1の樹脂層と第2の樹脂層とが形成されることとなる。   According to this invention, since the 1st resin composition which comprises the 1st resin layer, and the 2nd resin composition which comprises the 2nd resin layer are mutually different compositions, both surfaces of a prepreg In this case, a first resin layer and a second resin layer having different uses, functions, performances, and characteristics are formed.

また、本発明によれば、繊維基材を第1の樹脂層および第2の樹脂層で保護することができる。これにより、例えばプリプレグに外部からの衝撃が加わった場合でも、繊維基材自体が破壊するのが防止され、よって、繊維基材によるプリプレグの機械的強度を向上する効果が確実に発揮される。   Moreover, according to this invention, a fiber base material can be protected by the 1st resin layer and the 2nd resin layer. Thereby, for example, even when an external impact is applied to the prepreg, the fiber base material itself is prevented from being destroyed, and thus the effect of improving the mechanical strength of the prepreg by the fiber base material is reliably exhibited.

また、第1の樹脂層の第1の含浸部と第2の樹脂層の第2の含浸部とが密着するため、各樹脂層がそれぞれ繊維基材から剥離するのをより確実に防止することができる。これにより、プリプレグの耐久性の向上を図ることができる。   Moreover, since the 1st impregnation part of a 1st resin layer and the 2nd impregnation part of a 2nd resin layer closely_contact | adhere, it can prevent more reliably that each resin layer peels from a fiber base material, respectively. Can do. Thereby, the durability of the prepreg can be improved.

また、以上のような構成のプリプレグを備える基板を得、さらに、当該基板を用いて製造される半導体装置を得る。   Moreover, a board | substrate provided with the prepreg of the above structures is obtained, and also the semiconductor device manufactured using the said board | substrate is obtained.

本発明のプリプレグの実施形態を示す断面図である。It is sectional drawing which shows embodiment of the prepreg of this invention. 本発明の基板の実施形態を示す断面図である。It is sectional drawing which shows embodiment of the board | substrate of this invention. 本発明の半導体装置の実施形態を示す断面図である。It is sectional drawing which shows embodiment of the semiconductor device of this invention.

以下、本発明のプリプレグ、基板および半導体装置の好適実施形態について、添付図面に基づいて説明する。   Hereinafter, preferred embodiments of a prepreg, a substrate, and a semiconductor device of the present invention will be described with reference to the accompanying drawings.

図1は、本発明のプリプレグの実施形態を示す断面図、図2は、本発明の基板の実施形態を示す断面図、図3は、本発明の半導体装置の実施形態を示す断面図である。   1 is a cross-sectional view showing an embodiment of a prepreg of the present invention, FIG. 2 is a cross-sectional view showing an embodiment of a substrate of the present invention, and FIG. 3 is a cross-sectional view showing an embodiment of a semiconductor device of the present invention. .

<プリプレグ>
まず、本発明のプリプレグについて説明する。
<Prepreg>
First, the prepreg of the present invention will be described.

なお、以下の説明では、図1(以下の各図において同様)中の上側を「上」、下側を「下」として説明する。また、図1(以下の各図において同様)は、厚さ方向(図中の上下方向)に大きく誇張して示してある。   In the following description, the upper side in FIG. 1 (the same applies to the following drawings) is described as “upper”, and the lower side is described as “lower”. Further, FIG. 1 (same in the following drawings) is greatly exaggerated in the thickness direction (vertical direction in the drawing).

図1に示すプリプレグ1は、平板状の繊維基材2と、繊維基材2の一方の面(上面)側に位置する第1の樹脂層3と、繊維基材2の他方の面(下面)側に位置する第2の樹脂層4とを有する。
繊維基材2は、プリプレグ1の機械的強度を向上する機能を有する。
A prepreg 1 shown in FIG. 1 includes a flat fiber substrate 2, a first resin layer 3 positioned on one surface (upper surface) side of the fiber substrate 2, and the other surface (lower surface) of the fiber substrate 2. ) Side second resin layer 4.
The fiber base material 2 has a function of improving the mechanical strength of the prepreg 1.

この繊維基材2としては、例えば、ガラス織布、ガラス不織布等のガラス繊維基材、ポリアミド樹脂繊維、芳香族ポリアミド樹脂繊維、全芳香族ポリアミド樹脂繊維等のポリアミド系樹脂繊維、ポリエステル樹脂繊維、芳香族ポリエステル樹脂繊維、全芳香族ポリエステル樹脂繊維等のポリエステル系樹脂繊維、ポリイミド樹脂繊維、フッ素樹脂繊維等を主成分とする織布または不織布で構成される合成繊維基材、クラフト紙、コットンリンター紙、リンターとクラフトパルプの混抄紙等を主成分とする紙繊維基材等の有機繊維基材等の繊維基材等が挙げられる。   Examples of the fiber substrate 2 include glass fiber substrates such as glass woven fabric and glass nonwoven fabric, polyamide resin fibers, aromatic polyamide resin fibers, polyamide resin fibers such as wholly aromatic polyamide resin fibers, polyester resin fibers, Synthetic fiber substrate, kraft paper, cotton linter composed of woven or non-woven fabric mainly composed of aromatic polyester resin fiber, polyester resin fiber such as wholly aromatic polyester resin fiber, polyimide resin fiber, fluororesin fiber, etc. Examples thereof include fiber base materials such as organic fiber base materials such as paper fiber base materials mainly composed of paper, mixed paper of linter and kraft pulp, and the like.

これらの中でも、繊維基材2は、ガラス繊維基材であるのが好ましい。かかるガラス繊維基材を用いることにより、プリプレグ1の機械的強度をより向上することができる。また、プリプレグ1の熱膨張係数を小さくすることもできるという効果もある。   Among these, it is preferable that the fiber base material 2 is a glass fiber base material. By using such a glass fiber substrate, the mechanical strength of the prepreg 1 can be further improved. In addition, there is an effect that the thermal expansion coefficient of the prepreg 1 can be reduced.

このようなガラス繊維基材を構成するガラスとしては、例えば、Eガラス、Cガラス、Aガラス、Sガラス、Dガラス、NEガラス、Tガラス、Hガラス等が挙げられる。これらの中でも、ガラスは、Sガラス、または、Tガラスであるのが好ましい。これにより、ガラス繊維基材の熱膨張係数を比較的小さくすることができ、このため、プリプレグ1をその熱膨張係数ができる限り小さいものとすることができる。   As glass which comprises such a glass fiber base material, E glass, C glass, A glass, S glass, D glass, NE glass, T glass, H glass etc. are mentioned, for example. Among these, it is preferable that glass is S glass or T glass. Thereby, the thermal expansion coefficient of a glass fiber base material can be made comparatively small, and for this reason, the prepreg 1 can be made as small as possible in the thermal expansion coefficient.

繊維基材2の平均厚さは、特に限定されないが、150μm以下であるのが好ましく、100μm以下であるのがより好ましく、10〜50μm程度であるのがさらに好ましい。かかる厚さの繊維基材2を用いることにより、プリプレグ1の機械的強度を確保しつつ、その薄型化を図ることができる。さらには、プリプレグ1に対する孔あけ等の加工を施す際の加工性を向上することもできる。また、プリプレグ1を基板10にした状態で、当該基板10に対して、メカニカルドリルまたはレーザー照射による貫通孔(スルーホール)を加工する際の加工性も向上することができる。さらには、貫通孔同士間のピッチ間距離が70μm以下の狭ピッチにおける絶縁信頼性の向上を図ることもできる。   Although the average thickness of the fiber base material 2 is not specifically limited, It is preferable that it is 150 micrometers or less, It is more preferable that it is 100 micrometers or less, It is further more preferable that it is about 10-50 micrometers. By using the fiber substrate 2 having such a thickness, the mechanical strength of the prepreg 1 can be ensured and the thickness thereof can be reduced. Furthermore, workability when performing processing such as drilling on the prepreg 1 can be improved. Moreover, in the state which made the prepreg 1 the board | substrate 10, the workability at the time of processing the through-hole (through hole) by mechanical drill or laser irradiation with respect to the said board | substrate 10 can also be improved. Furthermore, it is possible to improve the insulation reliability at a narrow pitch where the distance between pitches between the through holes is 70 μm or less.

この繊維基材2の一方の面側には、第1の樹脂層3が設けられ、また、他方の面側には、第2の樹脂層4が設けられている。また、第1の樹脂層3は、第1の樹脂組成物で構成され、一方、第2の樹脂層4は、前記第1の樹脂組成物と異なる組成の第2の樹脂組成物で構成されている。   A first resin layer 3 is provided on one surface side of the fiber base 2, and a second resin layer 4 is provided on the other surface side. The first resin layer 3 is composed of a first resin composition, while the second resin layer 4 is composed of a second resin composition having a composition different from that of the first resin composition. ing.

かかる構成により、各樹脂層に要求される特性に応じて、樹脂組成物の組成を適宜設定することができるようになる。   With this configuration, the composition of the resin composition can be appropriately set according to the characteristics required for each resin layer.

本実施形態では、第1の樹脂層3上に配線部(導体パターン)を形成するために、第1の樹脂組成物は、金属との密着性に優れるような組成に設定されている。また、第2の樹脂層4に他のプリプレグ1の配線部や他の繊維基材を確実に埋め込むために、第2の樹脂組成物は、第2の樹脂層4が第1の樹脂層3より可撓性(柔軟性)が高くなるような組成に設定されている。このような各樹脂組成物については、後に詳述する。   In this embodiment, in order to form a wiring part (conductor pattern) on the 1st resin layer 3, the 1st resin composition is set to the composition which is excellent in adhesiveness with a metal. Moreover, in order to embed the wiring part of another prepreg 1 or another fiber base material in the second resin layer 4 reliably, the second resin layer 4 is composed of the first resin layer 3. The composition is set such that the flexibility (softness) is higher. Each such resin composition will be described in detail later.

図1に示すように、本発明では、繊維基材2の厚さ方向の一部に第1の樹脂組成物が含浸され(以下この部分を「第1の含浸部31」と言う)、繊維基材2の第1の樹脂組成物が含浸されていない残り部分に、第2の樹脂組成物が含浸されている(以下この部分を「第2の含浸部41」と言う)。これにより、第1の樹脂層3の一部である第1の含浸部31と第2の樹脂層4の一部である第2の含浸部41とが繊維基材2内に位置する。そして、繊維基材2内において、第1の含浸部31(第1の樹脂層3の下面)と第2の含浸部41(第2の樹脂層4の上面)とが接触している。換言すれば、本発明では、第1の樹脂組成物が、繊維基材2の上面側から、繊維基材2に含浸され、第2の樹脂組成物が、繊維基材2の下面側から、繊維基材2に含浸され、これらの樹脂組成物で繊維基材2内の空隙が充填されている。   As shown in FIG. 1, in the present invention, a part of the fiber base 2 in the thickness direction is impregnated with the first resin composition (hereinafter, this part is referred to as “first impregnation part 31”), and the fiber The remaining portion of the substrate 2 that is not impregnated with the first resin composition is impregnated with the second resin composition (hereinafter, this portion is referred to as “second impregnation portion 41”). Thereby, the first impregnation part 31 which is a part of the first resin layer 3 and the second impregnation part 41 which is a part of the second resin layer 4 are located in the fiber base material 2. And in the fiber base material 2, the 1st impregnation part 31 (lower surface of the 1st resin layer 3) and the 2nd impregnation part 41 (upper surface of the 2nd resin layer 4) are contacting. In other words, in the present invention, the first resin composition is impregnated into the fiber base material 2 from the upper surface side of the fiber base material 2, and the second resin composition is from the lower surface side of the fiber base material 2, The fiber base material 2 is impregnated, and the voids in the fiber base material 2 are filled with these resin compositions.

かかる構成により、繊維基材2を第1の樹脂層3および第2の樹脂層4で保護することができる。その結果、プリプレグ1に外部からの衝撃が加わった場合でも、繊維基材2自体が破壊するのを防止することができ、繊維基材2によるプリプレグ1の機械的強度を向上する効果を確実に発揮させることができる。   With this configuration, the fiber base 2 can be protected by the first resin layer 3 and the second resin layer 4. As a result, even when an external impact is applied to the prepreg 1, the fiber base material 2 itself can be prevented from being destroyed, and the effect of improving the mechanical strength of the prepreg 1 by the fiber base material 2 is ensured. It can be demonstrated.

また、繊維基材2内部における第1の含浸部31と第2の含浸部41との界面20を微視的に見た場合、この界面20は、凹凸をなすのが好ましい(図1中の拡大詳細図参照)。また、この界面20は、第1の含浸部31(第1の樹脂層3)と第2の樹脂層4とが互いに溶融し混ざりあっていてもよい。これにより、各樹脂層の繊維基材2に対するアンカー効果のみならず、樹脂層同士の密着性が高まり、各樹脂層が繊維基材2から剥離するのをより確実に防止することができる。これにより、プリプレグ1の耐久性の向上を図ることができる。さらには、プリプレグ1を基板10にした際に吸湿耐熱性の向上を図ることができる。   Further, when the interface 20 between the first impregnation portion 31 and the second impregnation portion 41 inside the fiber base 2 is viewed microscopically, it is preferable that the interface 20 is uneven (see FIG. 1). See enlarged detail view). Further, the interface 20 may be such that the first impregnation portion 31 (first resin layer 3) and the second resin layer 4 are melted and mixed with each other. Thereby, not only the anchor effect with respect to the fiber base material 2 of each resin layer but the adhesiveness of resin layers increases, and it can prevent more reliably that each resin layer peels from the fiber base material 2. FIG. Thereby, the durability of the prepreg 1 can be improved. Furthermore, when the prepreg 1 is used as the substrate 10, it is possible to improve the moisture absorption heat resistance.

かかる凹凸をなす界面20は、例えば、まず、第1の樹脂組成物のワニスを、繊維基材2の一方の面側に供給、含浸して、第1の樹脂層3を一旦形成する。その後、第2の樹脂組成物のワニスを、繊維基材2の他方の面側に供給、含浸して、第2の樹脂層4を形成することにより、確実に得ることができる。なお、各樹脂組成物の含浸の程度、すなわち、各含浸部の厚さは、例えば、含浸温度および含浸時間を適宜調整することにより所望の大きさに設定することができる。また、これらの樹脂層を形成する順序は、逆であってもよいことは言うまでもない。また、第1の樹脂層3または第2の樹脂層4のうちの少なくとも一方に、微小の無機フィラーや溶剤を適宜含ませることで、前記界面20の凹凸の形成、または、前記第1の含浸部31と第2の樹脂層4とが溶融して混ざり合う状態にすることができる。   For example, first, the first resin layer 3 is formed once by supplying and impregnating the varnish of the first resin composition to one surface side of the fiber base 2. Thereafter, the second resin composition varnish is supplied and impregnated on the other surface side of the fiber substrate 2 to form the second resin layer 4, so that it can be reliably obtained. The degree of impregnation of each resin composition, that is, the thickness of each impregnation part can be set to a desired size by appropriately adjusting the impregnation temperature and the impregnation time, for example. Needless to say, the order of forming these resin layers may be reversed. Further, by forming at least one of the first resin layer 3 or the second resin layer 4 appropriately with a minute inorganic filler or a solvent, formation of irregularities of the interface 20 or the first impregnation is performed. The part 31 and the second resin layer 4 can be melted and mixed.

また、先に形成する樹脂層のワニスを繊維基材2に供給する際には、ワニスを供給するのと反対側の面から吸引操作を行うようにしてもよい。これにより、当該樹脂層を構成する樹脂組成物が繊維基材2に確実に含浸し、その繊維基材2内に形成される界面20を荒らす、すなわち、凹凸が形成されたもの(粗面のもの)とすることができる。なお、当該樹脂組成物の含浸の程度は、例えば、吸引時間や吸引力を適宜調整することにより所望の大きさに設定することができる。また、繊維基材2に振動を与えつつ、ワニスを供給するようにしてもよい。   Moreover, when supplying the varnish of the resin layer formed previously to the fiber base material 2, you may make it perform suction operation from the surface on the opposite side to supplying a varnish. Thereby, the resin composition which comprises the said resin layer impregnates the fiber base material 2 reliably, and the interface 20 formed in the fiber base material 2 is roughened, ie, the unevenness | corrugation was formed (rough surface) Thing). The degree of impregnation of the resin composition can be set to a desired size by appropriately adjusting the suction time and suction force, for example. Moreover, you may make it supply a varnish, giving the fiber base material 2 a vibration.

前述したように、第2の樹脂層4の可撓性は、第1の樹脂層3よりも高くなっている。このような大小関係となっている場合、第1の含浸部31の平均厚さta1[μm]が、第2の含浸部41の平均厚さtb1[μm]より大きく(ta1>tb1)設定するのが好ましい。これは、次のような理由による。 As described above, the flexibility of the second resin layer 4 is higher than that of the first resin layer 3. In such a magnitude relationship, the average thickness t a1 [μm] of the first impregnation portion 31 is larger than the average thickness t b1 [μm] of the second impregnation portion 41 (t a1 > t b1 ) It is preferable to set. This is due to the following reason.

第2の樹脂層4の可撓性を、第1の樹脂層3より高く設定した場合、第2の樹脂層4の熱膨張率は、第1の樹脂層3より大きくなる傾向がある。このため、「ta1>tb1」とは反対の大小関係である「ta1<tb1」とすると、プリプレグ1が加熱されたとき、繊維基材2の内部では、第2の含浸部41が第1の含浸部31より大きく変形して、繊維基材2の部分で割れ(クラック)等が生じるおそれがある。この繊維基材2の部分での割れ等は、プリプレグ1全体に大きく影響を与え、プリプレグ1が使用に耐え得るものとならないおそれがある。 When the flexibility of the second resin layer 4 is set higher than that of the first resin layer 3, the thermal expansion coefficient of the second resin layer 4 tends to be larger than that of the first resin layer 3. Therefore, when the opposite of magnitude relation between "t a1> t b1", "t a1 <t b1", when the prepreg 1 is heated, the inside of the fiber substrate 2, a second impregnation portion 41 However, there is a possibility that the fiber substrate 2 is deformed to a greater extent than the first impregnated portion 31 and a crack (crack) or the like occurs in the fiber base material 2 portion. The crack or the like in the fiber base material 2 part greatly affects the entire prepreg 1 and the prepreg 1 may not be able to withstand use.

これに対して、「ta1>tb1」とすれば、上記の不都合が生じるのを解消、すなわち、プリプレグ1に割れ等が発生するのを防止または抑制することができる。これにより、プリプレグ1は、使用に耐え得るものとなる。 On the other hand, if “t a1 > t b1 ”, it is possible to eliminate the above inconvenience, that is, to prevent or suppress the occurrence of cracks or the like in the prepreg 1. Thereby, the prepreg 1 can endure use.

具体的には、繊維基材2の最大厚さをT[μm]としたとき、前記平均厚さta1は、0.50×T〜0.95×Tであるのが好ましく、0.7×T〜0.9×Tであるのがより好ましい。平均厚さta1をかかる範囲に設定することにより、各樹脂層が繊維基材2から剥離するのを確実に防止しつつ、プリプレグ1に反りが発生するのをより確実に防止または抑制することができる。 Specifically, when the maximum thickness of the fiber substrate 2 is T [μm], the average thickness t a1 is preferably 0.50 × T to 0.95 × T, and 0.7 It is more preferable that it is * T-0.9 * T. By setting the average thickness ta1 in such a range, it is possible to more reliably prevent or suppress warping of the prepreg 1 while reliably preventing each resin layer from peeling from the fiber base 2. Can do.

また、第1の樹脂層3の第1の含浸部31を除く部分(第1の非含浸部32)の平均厚さをta2[μm]とし、第2の樹脂層4の第2の含浸部41を除く部分(第2の非含浸部42)の平均厚さをtb2[μm]としたとき、1.2×ta2<tb2なる関係を満足するのが好ましく、2×ta2<tb2なる関係を満足するのがより好ましく、3×t<tなる関係を満足するのがさらに好ましい。かかる関係を満足することにより、プリプレグ1の上面側の部分に比較的高い剛性を付与することができるため、当該プリプレグ1の上面(第1の非含浸部32上)に配線部を高い加工性で形成することができる。一方、第2の樹脂層4は、高い可撓性と十分な厚さを有することができるため、当該第2の樹脂層4(第2の非含浸部42)に他のプリプレグ1の配線部や他の繊維基材を埋め込む際、当該埋め込みを確実に行なうことができる、すなわち、他のプリプレグ1の配線部や他の繊維基材に対する埋め込み性が向上する。 Further, the average thickness of the portion (the first non-impregnated portion 32) excluding the first impregnation portion 31 of the first resin layer 3 is set to ta2 [μm], and the second impregnation of the second resin layer 4 is performed. When the average thickness of the portion excluding the portion 41 (second non-impregnated portion 42) is t b2 [μm], it is preferable that the relationship 1.2 × t a2 <t b2 is satisfied and 2 × t a2 It is more preferable to satisfy the relationship <t b2, and it is even more preferable to satisfy the relationship 3 × t a <t b . By satisfying such a relationship, a relatively high rigidity can be imparted to the portion on the upper surface side of the prepreg 1, so that the wiring portion is highly workable on the upper surface of the prepreg 1 (on the first non-impregnated portion 32). Can be formed. On the other hand, since the second resin layer 4 can have high flexibility and sufficient thickness, the second resin layer 4 (second non-impregnated portion 42) is connected to the wiring portion of another prepreg 1. When embedding other fiber base materials, the embedding can be reliably performed, that is, the embedding property to the wiring part of other prepregs 1 or other fiber base materials is improved.

具体的には、平均厚さta2は、0.1〜15μmであるのが好ましく、1〜10μmであるのがより好ましい。一方、平均厚さtb2は、4〜50μmであるのが好ましく、8〜40μmであるのがより好ましい。 Specifically, the average thickness t a2 is preferably 0.1 to 15 μm, and more preferably 1 to 10 μm. On the other hand, the average thickness t b2 is preferably 4 to 50 μm, and more preferably 8 to 40 μm.

さて、上記の特性を有する第1の樹脂層3および第2の樹脂層4をそれぞれ得るために、第1の樹脂組成物および第2の樹脂組成物は、次のような組成とするのが好ましい。   Now, in order to obtain the 1st resin layer 3 and the 2nd resin layer 4 which have said characteristic, respectively, the 1st resin composition and the 2nd resin composition are set as the following compositions. preferable.

第1の樹脂組成物は、例えば、硬化性樹脂を含み、必要に応じて、硬化助剤(例えば硬化剤、硬化促進剤等)および無機充填材のうちの少なくとも1種を含んで構成される。   The first resin composition includes, for example, a curable resin, and includes at least one of a curing aid (for example, a curing agent and a curing accelerator) and an inorganic filler as necessary. .

配線部を構成する金属との密着性を向上させるには、金属との密着性に優れる硬化性樹脂を使用する方法、金属との密着性を向上させる硬化助剤(例えば硬化剤、硬化促進剤等)を使用する方法、無機充填材として酸に可溶なものを用いる方法、無機充填材と有機充填材とを併用する方法等が挙げられる。   In order to improve the adhesion with the metal constituting the wiring part, a method of using a curable resin excellent in adhesion with the metal, a curing aid for improving the adhesion with the metal (for example, a curing agent, a curing accelerator) Etc.), a method using an acid-soluble material as an inorganic filler, a method using an inorganic filler and an organic filler in combination, and the like.

かかる硬化性樹脂には、例えば、ユリア(尿素)樹脂、メラミン樹脂、ビスマレイミド樹脂、ポリウレタン樹脂、ベンゾオキサジン環を有する樹脂、シアネートエステル樹脂、ビスフェノールS型エポキシ樹脂、ビスフェノールF型エポキシ樹脂およびビスフェノールSとビスフェノールFとの共重合エポキシ樹脂等の熱硬化性樹脂が好適に用いられる。これらの中でも、硬化性樹脂には、特に、シアネート樹脂(シアネート樹脂のプレポリマーを含む)を用いるのが好ましい。   Examples of such curable resins include urea (urea) resins, melamine resins, bismaleimide resins, polyurethane resins, resins having a benzoxazine ring, cyanate ester resins, bisphenol S-type epoxy resins, bisphenol F-type epoxy resins, and bisphenol S. A thermosetting resin such as an epoxy resin copolymerized with bisphenol F is preferably used. Among these, it is particularly preferable to use a cyanate resin (including a prepolymer of cyanate resin) as the curable resin.

熱硬化性樹脂(特に、シアネート樹脂)を用いることにより、プリプレグ1の熱膨張係数を小さくすること(以下、「低熱膨張化」と言うこともある)ができる。さらに、プリプレグ1の電気特性(低誘電率、低誘電正接)等の向上を図ることもできる。   By using a thermosetting resin (particularly a cyanate resin), the coefficient of thermal expansion of the prepreg 1 can be reduced (hereinafter also referred to as “low thermal expansion”). Furthermore, the electrical characteristics (low dielectric constant, low dielectric loss tangent) of the prepreg 1 can be improved.

かかるシアネート樹脂は、例えば、ハロゲン化シアン化合物とフェノール類とを反応させ、必要に応じて、加熱等の方法でプレポリマー化することにより得ることができる。   Such a cyanate resin can be obtained, for example, by reacting a halogenated cyanide compound with a phenol and prepolymerizing it by a method such as heating, if necessary.

具体的なシアネート樹脂としては、例えば、ノボラック型シアネート樹脂、ビスフェノールA型シアネート樹脂、ビスフェノールE型シアネート樹脂、テトラメチルビスフェノールF型シアネート樹脂等のビスフェノール型シアネート樹脂等を挙げることができる。これらの中でも、シアネート樹脂は、ノボラック型シアネート樹脂であるのが好ましい。   Specific examples of the cyanate resin include novolac type cyanate resin, bisphenol A type cyanate resin, bisphenol E type cyanate resin, and bisphenol type cyanate resin such as tetramethylbisphenol F type cyanate resin. Among these, it is preferable that cyanate resin is a novolak-type cyanate resin.

ノボラック型シアネート樹脂を用いれば、後述する基板10(図2参照)を作製した後において、硬化後の第1の樹脂層3中において架橋密度が増加するので、硬化後の第1の樹脂層3(得られる基板)の耐熱性および難燃性の向上を図ることができる。   If a novolac-type cyanate resin is used, the cross-link density increases in the first resin layer 3 after curing after the substrate 10 (see FIG. 2) to be described later is manufactured, so the first resin layer 3 after curing. The heat resistance and flame retardance of the (obtained substrate) can be improved.

ここで、耐熱性の向上は、ノボラック型シアネート樹脂が硬化反応後にトリアジン環を形成することに起因すると考えられる。また、難燃性の向上は、ノボラック型シアネート樹脂がその構造上ベンゼン環の割合が高いため、このベンゼン環が炭化(グラファイト化)し易く、硬化後の第1の樹脂層3中に炭化部分が生じることに起因すると考えられる。   Here, it is considered that the improvement in heat resistance is caused by the novolak cyanate resin forming a triazine ring after the curing reaction. Further, the flame retardancy is improved because the novolak-type cyanate resin has a high proportion of benzene rings due to its structure, so that the benzene rings are easily carbonized (graphitized), and the first resin layer 3 after curing has a carbonized portion. This is thought to be caused by the occurrence of

さらに、ノボラック型シアネート樹脂を用いれば、プリプレグ1を薄型化(例えば、厚さ35μm以下)した場合であっても、プリプレグ1に優れた剛性を付与することができる。また、その硬化物は、加熱時における剛性にも優れるので、得られる基板10は、半導体素子500(図3参照)を実装する際の信頼性にも優れる。
具体的には、式(I)で示されるノボラック型シアネート樹脂を用いることができる。
Furthermore, if a novolac-type cyanate resin is used, even if the prepreg 1 is thinned (for example, 35 μm or less in thickness), excellent rigidity can be imparted to the prepreg 1. Moreover, since the cured product is excellent in rigidity at the time of heating, the obtained substrate 10 is also excellent in reliability when the semiconductor element 500 (see FIG. 3) is mounted.
Specifically, a novolac type cyanate resin represented by the formula (I) can be used.

Figure 0005552969
Figure 0005552969

式(I)で示されるノボラック型シアネート樹脂において、その平均繰り返し単位数「n」は、特に限定されないが、1〜10であるのが好ましく、2〜7であるのがより好ましい。平均繰り返し単位数「n」が前記下限値未満であると、ノボラック型シアネート樹脂は、結晶化し易くなるため、汎用溶媒に対する溶解性が低下する。このため、ノボラック型シアネート樹脂の含有量等によっては、第1の樹脂組成物のワニスが取り扱い難くなる場合がある。また、プリプレグ1を作製した場合にタック性が生じ、プリプレグ1同士が接触したとき互いに付着したり、一方のプリプレグ1の第1の樹脂組成物が他方のプリプレグ1に移行する現象(転写)が生じたりする場合がある。一方、平均繰り返し単位数「n」が前記上限値を超えると、第1の樹脂組成物のワニスの粘度が高くなりすぎ、プリプレグ1を作製する際の効率(第1の樹脂層3の成形性)が低下する場合がある。   In the novolak-type cyanate resin represented by the formula (I), the average number of repeating units “n” is not particularly limited, but is preferably 1 to 10, and more preferably 2 to 7. When the average number of repeating units “n” is less than the lower limit, the novolac cyanate resin is easily crystallized, and thus the solubility in a general-purpose solvent decreases. For this reason, depending on the content of the novolac-type cyanate resin, the varnish of the first resin composition may be difficult to handle. In addition, when the prepreg 1 is produced, tackiness occurs, and when the prepregs 1 come into contact with each other, a phenomenon (transfer) occurs in which the prepregs 1 adhere to each other or the first resin composition of one prepreg 1 moves to the other prepreg 1. May occur. On the other hand, if the average number of repeating units “n” exceeds the upper limit, the viscosity of the varnish of the first resin composition becomes too high, and the efficiency (the moldability of the first resin layer 3) when producing the prepreg 1 is increased. ) May decrease.

また、後述する金属との密着性を向上させる硬化剤または硬化促進剤を併用する場合には、上述の硬化性樹脂以外に、例えば、フェノールノボラック樹脂、クレゾールノボラック樹脂、ビスフェノールAノボラック樹脂等のノボラック型フェノール樹脂、未変性のレゾールフェノール樹脂、桐油、アマニ油、クルミ油等で変性した油変性レゾールフェノール樹脂等のレゾール型フェノール樹脂等のフェノール樹脂、ビスフェノールAエポキシ樹脂、ビスフェノールFエポキシ樹脂等のビスフェノール型エポキシ樹脂、ノボラックエポキシ樹脂、クレゾールノボラックエポキシ樹脂等のノボラック型エポキシ樹脂、ビフェニル型エポキシ樹脂等のエポキシ樹脂、不飽和ポリエステル樹脂、ジアリルフタレート樹脂、シリコーン樹脂等の他の熱硬化性樹脂を用いることもできる。   Moreover, when using together the hardening | curing agent or hardening accelerator which improves the adhesiveness with the metal mentioned later, novolaks, such as a phenol novolak resin, a cresol novolak resin, a bisphenol A novolak resin other than the above-mentioned curable resin, for example. Type phenolic resin, unmodified resol phenolic resin, phenolic resin such as oil-modified resol phenolic resin modified with tung oil, linseed oil, walnut oil, etc., bisphenol such as bisphenol A epoxy resin, bisphenol F epoxy resin Other epoxy resins such as epoxy resin such as epoxy resin, novolak epoxy resin, novolac epoxy resin such as cresol novolak epoxy resin, epoxy resin such as biphenyl epoxy resin, unsaturated polyester resin, diallyl phthalate resin, silicone resin It can also be used RESIN.

さらに、硬化性樹脂には、熱硬化性樹脂の他、例えば、紫外線硬化性樹脂、嫌気硬化性樹脂等を用いることもできる。   In addition to the thermosetting resin, for example, an ultraviolet curable resin, an anaerobic curable resin, or the like can be used as the curable resin.

硬化性樹脂の含有量は、特に限定されないが、第1の樹脂組成物全体の5〜50重量%であるのが好ましく、10〜40重量%であるのがより好ましい。硬化性樹脂の含有量が前記下限値未満であると、硬化性樹脂の種類等によっては、第1の樹脂組成物のワニスの粘度が低くなりすぎ、プリプレグ1を形成するのが困難となる場合がある。一方、硬化性樹脂の含有量が前記上限値を超えると、他の成分の量が少なくなり過ぎるため、硬化性樹脂の種類等によっては、プリプレグ1の機械的強度が低下する場合がある。   Although content of curable resin is not specifically limited, It is preferable that it is 5 to 50 weight% of the whole 1st resin composition, and it is more preferable that it is 10 to 40 weight%. When the content of the curable resin is less than the lower limit, depending on the type of the curable resin, the viscosity of the varnish of the first resin composition becomes too low and it is difficult to form the prepreg 1. There is. On the other hand, when the content of the curable resin exceeds the upper limit, the amount of other components is too small, and the mechanical strength of the prepreg 1 may be reduced depending on the type of the curable resin.

上述の硬化助剤(例えば硬化剤、硬化促進剤等)としては、例えば、トリエチルアミン、トリブチルアミン、ジアザビシクロ[2,2,2]オクタン等の3級アミン類、2−エチル−4−エチルイミダゾール、2−フェニル−4−メチルイミダゾール、2−フェニル−4−メチル−5−ヒドルキシメチルイミダゾール、2−フェニル−4,5−ジヒドロキシメチルイミダゾール、2,4−ジアミノ−6−〔2’−メチルイミダゾリル−(1’)〕−エチル−s−トリアジン、2,4−ジアミノ−6−(2’−ウンデシルイミダゾリル)−エチル−s−トリアジン、2,4−ジアミノ−6−〔2’−エチル−4−メチルイミダゾリル−(1’)〕−エチル−s−トリアジン、1−ベンジル−2−フェニルイミダゾール等のイミダゾール化合物が挙げられる。   Examples of the above-described curing aid (for example, a curing agent, a curing accelerator, etc.) include tertiary amines such as triethylamine, tributylamine, diazabicyclo [2,2,2] octane, 2-ethyl-4-ethylimidazole, 2-phenyl-4-methylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2-phenyl-4,5-dihydroxymethylimidazole, 2,4-diamino-6- [2'-methyl Imidazolyl- (1 ′)]-ethyl-s-triazine, 2,4-diamino-6- (2′-undecylimidazolyl) -ethyl-s-triazine, 2,4-diamino-6- [2′-ethyl Imidazole compounds such as -4-methylimidazolyl- (1 ′)]-ethyl-s-triazine and 1-benzyl-2-phenylimidazole It is below.

これらの中でも、硬化助剤は、脂肪族炭化水素基、芳香族炭化水素基、ヒドロキシアルキル基およびシアノアルキル基の中から選ばれる官能基を2個以上有しているイミダゾール化合物であるのが好ましく、2−フェニル−4,5−ジヒドロキシメチルイミダゾールであるのがより好ましい。   Among these, the curing aid is preferably an imidazole compound having two or more functional groups selected from an aliphatic hydrocarbon group, an aromatic hydrocarbon group, a hydroxyalkyl group, and a cyanoalkyl group. 2-phenyl-4,5-dihydroxymethylimidazole is more preferable.

また、第1の樹脂組成物には、例えば、ナフテン酸亜鉛、ナフテン酸コバルト、オクチル酸スズ、オクチル酸コバルト、ビスアセチルアセトナートコバルト(II)、トリスアセチルアセトナートコバルト(III)等の有機金属塩、フェノール、ビスフェノールA、ノニルフェノール等のフェノール化合物、酢酸、安息香酸、サリチル酸、パラトルエンスルホン酸等の有機酸等を組み合わせて用いることができる。   Examples of the first resin composition include organic metals such as zinc naphthenate, cobalt naphthenate, tin octylate, cobalt octylate, bisacetylacetonate cobalt (II), and trisacetylacetonate cobalt (III). A salt, a phenol compound such as phenol, bisphenol A, and nonylphenol, an organic acid such as acetic acid, benzoic acid, salicylic acid, and paratoluenesulfonic acid can be used in combination.

硬化助剤を用いる場合、その含有量は、第1の樹脂組成物全体の0.01〜3重量%であるのが好ましく、0.1〜1重量%であるのがより好ましい。   When using a curing aid, its content is preferably 0.01 to 3% by weight, more preferably 0.1 to 1% by weight of the entire first resin composition.

また、第1の樹脂組成物は、無機充填材を含むことが好ましい。これにより、プリプレグ1を薄型化(例えば、厚さ35μm以下)にしても、機械的強度に優れるプリプレグ1を得ることができる。さらに、プリプレグ1の低熱膨張化を向上することもできる。   Moreover, it is preferable that a 1st resin composition contains an inorganic filler. Thereby, even if the prepreg 1 is made thin (for example, a thickness of 35 μm or less), the prepreg 1 having excellent mechanical strength can be obtained. Furthermore, the low thermal expansion of the prepreg 1 can be improved.

無機充填材としては、例えば、タルク、アルミナ、ガラス、溶融シリカのようなシリカ、マイカ、水酸化アルミニウム、水酸化マグネシウム等を挙げることができる。また、無機充填材の使用目的に応じて、破砕状、球状のものが適宜選択される。これらの中でも、低熱膨張性に優れる観点からは、無機充填剤は、シリカであるのが好ましく、溶融シリカ(特に球状溶融シリカ)であるのがより好ましい。   Examples of the inorganic filler include talc, alumina, glass, silica such as fused silica, mica, aluminum hydroxide, magnesium hydroxide and the like. Further, depending on the purpose of use of the inorganic filler, a crushed or spherical one is appropriately selected. Among these, from the viewpoint of excellent low thermal expansibility, the inorganic filler is preferably silica, and more preferably fused silica (particularly spherical fused silica).

無機充填材の平均粒径は、0.01〜5.0μmであるのが好ましく、0.2〜2.0μmであるのがより好ましい。なお、この平均粒径は、例えば、粒度分布計(HORIBA製「LA−500」)により測定することができる。   The average particle size of the inorganic filler is preferably 0.01 to 5.0 μm, and more preferably 0.2 to 2.0 μm. In addition, this average particle diameter can be measured with a particle size distribution meter (“LA-500” manufactured by HORIBA), for example.

特に、無機充填材としては、平均粒径5.0μm以下の球状溶融シリカが好ましく、平均粒子径0.01〜2.0μm(特に、0.1〜0.5μm)の球状溶融シリカがより好ましい。これにより、第1の樹脂組成物のワニスを繊維基材2内により確実に含浸させることができ、また、形成された第1の樹脂層3(第1の含浸部31)の繊維基材2の内部における面に凹凸をより確実に形成することができる。   In particular, as the inorganic filler, spherical fused silica having an average particle diameter of 5.0 μm or less is preferable, and spherical fused silica having an average particle diameter of 0.01 to 2.0 μm (particularly 0.1 to 0.5 μm) is more preferable. . Thereby, the varnish of the 1st resin composition can be more reliably impregnated in the fiber base material 2, and the fiber base material 2 of the formed 1st resin layer 3 (1st impregnation part 31). Unevenness can be more reliably formed on the surface inside the.

また、第1の樹脂層3と配線部との密着性を向上するために、無機充填材として、酸に可溶な無機充填材を用いてもよい。これにより、配線部(導体層)を第1の樹脂層3上にメッキ法で形成した場合に、その配線部の第1の樹脂層3に対する密着性(メッキ密着性)を向上することができる。この酸に可溶な無機充填材としては、例えば、炭酸カルシウム、酸化亜鉛、酸化鉄等の金属酸化物等が挙げられる。   Moreover, in order to improve the adhesiveness of the 1st resin layer 3 and a wiring part, you may use an inorganic filler soluble in an acid as an inorganic filler. Thereby, when the wiring part (conductor layer) is formed on the first resin layer 3 by plating, the adhesion (plating adhesion) of the wiring part to the first resin layer 3 can be improved. . Examples of the acid-soluble inorganic filler include metal oxides such as calcium carbonate, zinc oxide, and iron oxide.

また、第1の樹脂層3と配線部との密着性を向上するために、無機充填材と有機充填材とを併用してもよい。この有機充填材としては、例えば、液晶ポリマー、ポリイミド等の樹脂系充填材が挙げられる。   Moreover, in order to improve the adhesiveness of the 1st resin layer 3 and a wiring part, you may use together an inorganic filler and an organic filler. Examples of the organic filler include resin fillers such as liquid crystal polymer and polyimide.

無機充填材を用いる場合、その含有量は、特に限定されないが、第1の樹脂組成物全体の20〜70重量%であるのが好ましく、30〜60重量%であるのがより好ましい。   When the inorganic filler is used, the content thereof is not particularly limited, but is preferably 20 to 70% by weight, more preferably 30 to 60% by weight of the entire first resin composition.

硬化性樹脂としてシアネート樹脂(特に、ノボラック型シアネート樹脂)を用いる場合には、エポキシ樹脂(実質的にハロゲン原子を含まない)を併用することが好ましい。このエポキシ樹脂としては、例えば、フェノールノボラック型エポキシ樹脂、ビスフェノール型エポキシ樹脂、ナフタレン型エポキシ樹脂、アリールアルキレン型エポキシ樹脂等が挙げられる。   When a cyanate resin (particularly a novolak cyanate resin) is used as the curable resin, it is preferable to use an epoxy resin (substantially free of halogen atoms) in combination. Examples of the epoxy resin include phenol novolac type epoxy resin, bisphenol type epoxy resin, naphthalene type epoxy resin, arylalkylene type epoxy resin, and the like.

これらの中でも、エポキシ樹脂は、アリールアルキレン型エポキシ樹脂であるのが好ましい。アリールアルキレン型エポキシ樹脂を用いることにより、硬化後の第1の樹脂層3(得られる基板)において、吸湿半田耐熱性(吸湿後の半田耐熱性)および難燃性を向上させることができる。   Among these, the epoxy resin is preferably an aryl alkylene type epoxy resin. By using the aryl alkylene type epoxy resin, it is possible to improve the moisture absorption solder heat resistance (solder heat resistance after moisture absorption) and flame retardancy in the cured first resin layer 3 (obtained substrate).

アリールアルキレン型エポキシ樹脂とは、繰り返し単位中に一つ以上のアリールアルキレン基を有するエポキシ樹脂をいい、例えば、キシリレン型エポキシ樹脂、ビフェニルジメチレン型エポキシ樹脂等が挙げられる。これらの中でも、アリールアルキレン型エポキシ樹脂は、ビフェニルジメチレン型エポキシ樹脂であるのが好ましい。   The aryl alkylene type epoxy resin refers to an epoxy resin having one or more aryl alkylene groups in the repeating unit, and examples thereof include a xylylene type epoxy resin and a biphenyl dimethylene type epoxy resin. Among these, the aryl alkylene type epoxy resin is preferably a biphenyl dimethylene type epoxy resin.

具体的には、式(II)で示されるビフェニルジメチレン型エポキシ樹脂を用いることができる。   Specifically, a biphenyl dimethylene type epoxy resin represented by the formula (II) can be used.

Figure 0005552969
Figure 0005552969

式(II)で示されるビフェニルジメチレン型エポキシ樹脂の平均繰り返し単位数「n」は、特に限定されないが、1〜10であるのが好ましく、2〜5であるのがより好ましい。平均繰り返し単位数「n」が前記下限値未満であると、ビフェニルジメチレン型エポキシ樹脂は、結晶化し易くなるため、汎用溶媒に対する溶解性が低下する。このため、第1の樹脂組成物のワニスが取り扱い難くなる場合がある。一方、平均繰り返し単位数「n」が前記上限値を超えると、用いる溶媒によっては、第1の樹脂組成物のワニスの粘度が上昇する恐れがある。この場合、第1の樹脂組成物を繊維基材2に十分に含浸できず、結果として、プリプレグ1の成形不良や機械的強度の低下の原因となることがある。   The average number of repeating units “n” of the biphenyl dimethylene type epoxy resin represented by the formula (II) is not particularly limited, but is preferably 1 to 10, and more preferably 2 to 5. When the average number of repeating units “n” is less than the lower limit, the biphenyldimethylene type epoxy resin is easily crystallized, so that the solubility in a general-purpose solvent decreases. For this reason, the varnish of the first resin composition may be difficult to handle. On the other hand, if the average number of repeating units “n” exceeds the upper limit, depending on the solvent used, the viscosity of the varnish of the first resin composition may increase. In this case, the fiber base material 2 cannot be sufficiently impregnated with the first resin composition, and as a result, the molding failure of the prepreg 1 and the mechanical strength may be reduced.

エポキシ樹脂を併用する場合、その含有量は、特に限定されないが、第1の樹脂組成物全体の1〜55重量%であるのが好ましく、2〜40重量%であるのがより好ましい。   When the epoxy resin is used in combination, the content is not particularly limited, but it is preferably 1 to 55% by weight, more preferably 2 to 40% by weight based on the entire first resin composition.

さらに、第1の樹脂組成物には、金属との密着性が向上するような成分(樹脂等を含む)を添加してもよい。かかる成分としては、例えば、フェノキシ樹脂、ポリビニルアルコール系樹脂、カップリング剤等が挙げられる。   Furthermore, you may add to a 1st resin composition the component (a resin etc. are included) which improves adhesiveness with a metal. Examples of such components include phenoxy resins, polyvinyl alcohol resins, coupling agents, and the like.

フェノキシ樹脂としては、例えば、ビスフェノール骨格を有するフェノキシ樹脂、ナフタレン骨格を有するフェノキシ樹脂、ビフェニル骨格を有するフェノキシ樹脂等が挙げられる。また、これらの骨格を複数種有した構造のフェノキシ樹脂を用いることもできる。   Examples of the phenoxy resin include a phenoxy resin having a bisphenol skeleton, a phenoxy resin having a naphthalene skeleton, and a phenoxy resin having a biphenyl skeleton. A phenoxy resin having a structure having a plurality of these skeletons can also be used.

これらの中でも、フェノキシ樹脂には、ビフェニル骨格およびビスフェノールS骨格を有するフェノキシ樹脂を用いるのが好ましい。これにより、ビフェニル骨格が有する剛直性により、フェノキシ樹脂のガラス転移温度を高くすることができるとともに、ビスフェノールS骨格の存在により、フェノキシ樹脂の金属との密着性を向上させることができる。その結果、第1の樹脂層3の耐熱性の向上を図ることができるとともに、多層基板を製造する際に、第1の樹脂層3に対する配線部(金属)の密着性を向上させることができる。   Among these, it is preferable to use a phenoxy resin having a biphenyl skeleton and a bisphenol S skeleton as the phenoxy resin. Accordingly, the glass transition temperature of the phenoxy resin can be increased due to the rigidity of the biphenyl skeleton, and the adhesion of the phenoxy resin to the metal can be improved due to the presence of the bisphenol S skeleton. As a result, the heat resistance of the first resin layer 3 can be improved, and the adhesion of the wiring part (metal) to the first resin layer 3 can be improved when a multilayer substrate is manufactured. .

また、フェノキシ樹脂には、ビスフェノールA骨格およびビスフェノールF骨格を有するフェノキシ樹脂を用いるのも好ましい。これにより、多層基板の製造時に、配線部の第1の樹脂層3への密着性をさらに向上させることができる。   It is also preferable to use a phenoxy resin having a bisphenol A skeleton and a bisphenol F skeleton as the phenoxy resin. Thereby, the adhesiveness to the 1st resin layer 3 of a wiring part can be further improved at the time of manufacture of a multilayer substrate.

フェノキシ樹脂の分子量は、特に限定されないが、重量平均分子量が5,000〜70,000であるのが好ましく、10,000〜60,000であるのがより好ましい。   The molecular weight of the phenoxy resin is not particularly limited, but the weight average molecular weight is preferably 5,000 to 70,000, and more preferably 10,000 to 60,000.

フェノキシ樹脂を用いる場合、その含有量は、特に限定されないが、第1の樹脂組成物全体の1〜40重量%であるのが好ましく、5〜30重量%であるのがより好ましい。   When the phenoxy resin is used, its content is not particularly limited, but it is preferably 1 to 40% by weight, more preferably 5 to 30% by weight based on the entire first resin composition.

カップリング剤には、例えば、エポキシシランカップリング剤、チタネート系カップリング剤、アミノシランカップリング剤およびシリコーンオイル型カップリング剤の中から選ばれる1種以上を用いるのが好ましい。   As the coupling agent, it is preferable to use at least one selected from, for example, an epoxy silane coupling agent, a titanate coupling agent, an aminosilane coupling agent, and a silicone oil type coupling agent.

カップリング剤を用いる場合、その含有量は、特に限定されないが、無機充填材100重量部に対して0.05〜3重量部であるのが好ましく、0.1〜2重量部であるのがより好ましい。   When using a coupling agent, the content is not particularly limited, but it is preferably 0.05 to 3 parts by weight, and 0.1 to 2 parts by weight with respect to 100 parts by weight of the inorganic filler. More preferred.

また、第1の樹脂組成物は、以上に説明した成分のほか、必要に応じて消泡剤、レベリング剤、顔料、酸化防止剤等の添加剤を含有することができる。   Moreover, the 1st resin composition can contain additives, such as an antifoamer, a leveling agent, a pigment, antioxidant, as needed besides the component demonstrated above.

第2の樹脂組成物は、第1の樹脂組成物と異なる組成、具体的には、第2の樹脂層4が第1の樹脂層3より可撓性が高くなるような組成に設定されている。   The second resin composition is set to a composition different from the first resin composition, specifically, a composition in which the second resin layer 4 is more flexible than the first resin layer 3. Yes.

第2の樹脂組成物の構成成分には、第1の樹脂組成物で挙げたものと同様のものを用いることができるが、樹脂や充填材等の種類および含有量、樹脂の分子量(平均繰り返し単位数)等の少なくとも1つを異ならせることにより、第2の樹脂組成物の組成は、第1の樹脂組成物と異なっている。その結果、第2の樹脂層4は、第1の樹脂層3と異なる特性を有している。   The constituents of the second resin composition can be the same as those mentioned in the first resin composition, but the type and content of the resin and filler, the molecular weight of the resin (average repeat The composition of the second resin composition differs from that of the first resin composition by making at least one such as the number of units different. As a result, the second resin layer 4 has different characteristics from the first resin layer 3.

この第2の樹脂層4の面方向、すなわち、プリプレグ1の長手方向(X方向)および幅方向(Y方向)の熱膨張係数は、特に限定されないが、20ppm以下であるのが好ましく、5〜16ppmであるのがより好ましい。第2の樹脂層4の熱膨張係数が前記範囲内であると、プリプレグ1は、高い接続信頼性を有すことができ、得られる基板は、半導体素子等の実装信頼性に優れたものとなる。   The thermal expansion coefficient in the surface direction of the second resin layer 4, that is, the longitudinal direction (X direction) and the width direction (Y direction) of the prepreg 1 is not particularly limited, but is preferably 20 ppm or less, More preferably, it is 16 ppm. When the thermal expansion coefficient of the second resin layer 4 is within the above range, the prepreg 1 can have high connection reliability, and the obtained substrate is excellent in mounting reliability of semiconductor elements and the like. Become.

また、プリプレグ1全体の面方向の熱膨張係数は、特に限定されないが、16ppm以下であるのが好ましく、12ppm以下であるのがより好ましく、5〜10ppmであるのがさらに好ましい。プリプレグ1の熱膨張係数が前記範囲内であると、得られる基板において、繰り返しの熱衝撃に対する耐クラック性が向上する。   Further, the thermal expansion coefficient in the plane direction of the entire prepreg 1 is not particularly limited, but is preferably 16 ppm or less, more preferably 12 ppm or less, and further preferably 5 to 10 ppm. When the thermal expansion coefficient of the prepreg 1 is within the above range, the crack resistance to repeated thermal shocks is improved in the obtained substrate.

面方向の熱膨張係数は、例えば、TMA装置(TAインスツルメント社製)を用いて、10℃/分で昇温して評価することができる。   The thermal expansion coefficient in the surface direction can be evaluated by increasing the temperature at 10 ° C./min using, for example, a TMA apparatus (TA Instruments).

<基板>
次に、本発明の基板について、図2を参照しつつ説明する。この図2に示す基板10は、積層体11と、この積層体11の両面に設けられた金属層12とを有している。
<Board>
Next, the substrate of the present invention will be described with reference to FIG. A substrate 10 shown in FIG. 2 includes a laminate 11 and metal layers 12 provided on both surfaces of the laminate 11.

積層体11は、第2の樹脂層4同士を内側にして配置された2つのプリプレグ1と、第2の樹脂層4同士間で挟持された繊維基材13とを備える。   The laminate 11 includes two prepregs 1 arranged with the second resin layers 4 facing each other, and a fiber base material 13 sandwiched between the second resin layers 4.

繊維基材13には、前述した繊維基材2と同様のものを用いることができる。また、本実施形態では、第2の樹脂層4は、前述したような特性(可撓性)を有するため、繊維基材13の少なくとも一部は、第2の樹脂層4に確実に埋め込まれる(埋設される)。   As the fiber base material 13, the same fiber base material 2 as described above can be used. In the present embodiment, since the second resin layer 4 has the characteristics (flexibility) as described above, at least a part of the fiber base material 13 is reliably embedded in the second resin layer 4. (Buried).

金属層12は、配線部に加工される部分であり、例えば、銅箔、アルミ箔等の金属箔を積層体11に接合すること、銅、アルミニウムを積層体11の表面にメッキすること等により形成される。また、本実施形態では、第1の樹脂層3は、前述したような特性を有するため、高い密着性で金属層12を保持することができるとともに、高い加工精度で金属層12を配線部に形成することができるようになっている。   The metal layer 12 is a part that is processed into a wiring part, for example, by bonding a metal foil such as a copper foil or an aluminum foil to the laminate 11, or plating copper or aluminum on the surface of the laminate 11. It is formed. In the present embodiment, since the first resin layer 3 has the characteristics as described above, the metal layer 12 can be held with high adhesion and the metal layer 12 can be used as a wiring portion with high processing accuracy. It can be formed.

金属層12と第1の樹脂層3とのピール強度は、0.5kN/m以上であるのが好ましく、0.6kN/m以上であるのがより好ましい。これにより、金属層12を配線部に加工し、得られる半導体装置100(図3参照)における接続信頼性をより向上させることができる。   The peel strength between the metal layer 12 and the first resin layer 3 is preferably 0.5 kN / m or more, and more preferably 0.6 kN / m or more. Thereby, the connection reliability in the semiconductor device 100 (refer FIG. 3) obtained by processing the metal layer 12 into a wiring part can be improved more.

このような基板10は、第1の樹脂層3上に金属層12を形成したプリプレグ1を2つ用意し、これらのプリプレグ1で繊維基材13を挟持した状態で、例えば、真空プレス、常圧ラミネータおよび真空下で加熱加圧するラミネータを用いて積層する方法が挙げられる。真空プレスは、平板に挟んで通常のホットプレス機等で実施できる。例えば、名機製作所社製の真空プレス、北川精機社製の真空プレス、ミカドテクノス社製の真空プレス等が挙げられる。また、ラミネータ装置としては、ニチゴー・モートン社製のバキュームアップリケーター、名機製作所社製の真空加圧式ラミネータ、日立テクノエンジニアリング社製の真空ロール式ドライコータ等のような市販の真空積層機、またはベルトプレス等を用いて製造することができる。   In such a substrate 10, two prepregs 1 each having a metal layer 12 formed on the first resin layer 3 are prepared, and the fiber base material 13 is sandwiched between these prepregs 1. Examples thereof include a method of laminating using a pressure laminator and a laminator heated and pressurized under vacuum. The vacuum press can be performed with a normal hot press machine or the like sandwiched between flat plates. For example, a vacuum press manufactured by Meiki Seisakusho Co., Ltd., a vacuum press manufactured by Kitagawa Seiki Co., Ltd., a vacuum press manufactured by Mikado Technos, etc. Further, as a laminator apparatus, a commercially available vacuum laminating machine such as a vacuum applicator manufactured by Nichigo Morton, a vacuum pressurizing laminator manufactured by Meiki Seisakusho, a vacuum roll type dry coater manufactured by Hitachi Techno Engineering, or the like It can be manufactured using a belt press or the like.

なお、本発明の基板10は、繊維基材13が省略され、2つのプリプレグ1が第2の樹脂層4同士を直接接合してなる積層体を含むものであってもよく、金属層12が省略されたものであってもよい。   The substrate 10 of the present invention may include a laminate in which the fiber base material 13 is omitted, and the two prepregs 1 are formed by directly joining the second resin layers 4 together. It may be omitted.

<半導体装置>
次に、本発明の半導体装置について、図3を参照しつつ説明する。なお、図3中では、繊維基材2、13を省略して示し、第1の樹脂層3および第2の樹脂層4を一体として示してある。
<Semiconductor device>
Next, the semiconductor device of the present invention will be described with reference to FIG. In FIG. 3, the fiber base materials 2 and 13 are omitted, and the first resin layer 3 and the second resin layer 4 are shown as an integral unit.

図3に示す半導体装置100は、多層基板200と、多層基板200の上面に設けられたパッド部300と、多層基板200の下面に設けられた配線部400と、パッド部300にバンプ501を接続することにより、多層基板200上に搭載された半導体素子500とを有している。また、その他、多層基板200の下面には、配線部、パッド部、半田ボール等が設けられていてもよい。   The semiconductor device 100 shown in FIG. 3 connects the bump 501 to the multilayer substrate 200, the pad portion 300 provided on the upper surface of the multilayer substrate 200, the wiring portion 400 provided on the lower surface of the multilayer substrate 200, and the pad portion 300. Thus, the semiconductor element 500 mounted on the multilayer substrate 200 is provided. In addition, a wiring part, a pad part, a solder ball, and the like may be provided on the lower surface of the multilayer substrate 200.

多層基板200は、コア基板として設けられた基板10と、この基板10の上側に設けられた3つのプリプレグ1a、1b、1cと、基板10の下側に設けられた3つのプリプレグ1d、1e、1fとを備えている。プリプレグ1a〜1cをそれぞれ構成する繊維基材2、第1の樹脂層3、第2の樹脂層4の基板10からの配置順番と、プリプレグ1d〜1fをそれぞれ構成する繊維基材2、第1の樹脂層3、第2の樹脂層4の基板10からの配置順番とは、同じとなっている。すなわち、プリプレグ1a〜1cとプリプレグ1d〜1fとは、互いに上下反転したもの同士となっている。   The multilayer substrate 200 includes a substrate 10 provided as a core substrate, three prepregs 1a, 1b, 1c provided on the upper side of the substrate 10, and three prepregs 1d, 1e provided on the lower side of the substrate 10. 1f. The fiber base material 2, the first resin layer 3, and the second resin layer 4 constituting the prepregs 1a to 1c, respectively, from the substrate 10, the fiber base material 2 constituting the prepregs 1d to 1f, the first The arrangement order of the resin layer 3 and the second resin layer 4 from the substrate 10 is the same. That is, the prepregs 1a to 1c and the prepregs 1d to 1f are inverted from each other.

また、多層基板200は、プリプレグ1aとプリプレグ1bとの間に設けられた回路部201aと、プリプレグ1bとプリプレグ1cとの間に設けられた回路部201bと、プリプレグ1dとプリプレグ1eとの間に設けられた回路部201dと、プリプレグ1eとプリプレグ1fとの間に設けられた回路部201eとを有している。   The multilayer substrate 200 includes a circuit unit 201a provided between the prepreg 1a and the prepreg 1b, a circuit unit 201b provided between the prepreg 1b and the prepreg 1c, and a prepreg 1d and the prepreg 1e. The circuit portion 201d is provided, and the circuit portion 201e is provided between the prepreg 1e and the prepreg 1f.

さらに、多層基板200は、各プリプレグ1a〜1fをそれぞれ貫通して設けられ、隣接する回路部同士や、回路部とパッド部とを電気的に接続する導体部202とを備えている。   Furthermore, the multilayer substrate 200 is provided through each of the prepregs 1a to 1f, and includes a conductor portion 202 that electrically connects adjacent circuit portions or between the circuit portion and the pad portion.

基板10の各金属層12は、それぞれ、所定のパターンに加工され、当該加工された金属層12同士は、基板10を貫通して設けられた導体部203により電気的に接続されている。   Each metal layer 12 of the substrate 10 is processed into a predetermined pattern, and the processed metal layers 12 are electrically connected to each other by a conductor portion 203 provided through the substrate 10.

なお、半導体装置100(多層基板200)は、基板10の片面側に、4つ以上のプリプレグ1を設けるようにしてもよい。さらに、半導体装置100は、本発明のプリプレグ1以外のプリプレグを含んでいてもよい。   In the semiconductor device 100 (multilayer substrate 200), four or more prepregs 1 may be provided on one side of the substrate 10. Furthermore, the semiconductor device 100 may include a prepreg other than the prepreg 1 of the present invention.

以上、本発明のプリプレグ、基板および半導体装置を図示の実施形態について説明したが、本発明は、これに限定されるものではなく、プリプレグ、基板および半導体装置を構成する各部は、同様の機能を発揮し得る任意の構成のものと置換することができる。また、任意の構成物が付加されていてもよい。   As described above, the prepreg, the substrate, and the semiconductor device of the present invention have been described with respect to the illustrated embodiment. However, the present invention is not limited to this, and the respective parts constituting the prepreg, the substrate, and the semiconductor device have the same functions. It can be replaced with any configuration that can be exhibited. Moreover, arbitrary components may be added.

また、プリプレグは、図1に示す構成では平均厚さta1と平均厚さtb1との大小関係はta1>tb1であるが、これとは反対の大小関係である「ta1<tb1」とした場合、プリプレグ1に反りが発生するのを防止または抑制することが可能である。 In the configuration shown in FIG. 1, the prepreg has a magnitude relationship between the average thickness t a1 and the average thickness t b1 that satisfies t a1 > t b1 , but the opposite magnitude relationship is “t a1 <t Whenb1 ” is set, warping of the prepreg 1 can be prevented or suppressed.

また、プリプレグは、図1に示す構成では平均厚さta2と平均厚さtb2との大小関係はta2<tb2であるが、これに限定されず、例えば、ta2>tb2であってもよいし、ta2=tb2であってもよい。 In the configuration shown in FIG. 1, the prepreg has a magnitude relationship between the average thickness t a2 and the average thickness t b2 that is t a2 <t b2 , but is not limited thereto, and for example, t a2 > t b2 Or t a2 = t b2 .

1、1a、1b、1c、1d、1e、1f プリプレグ
2 繊維基材
3 第1の樹脂層
31 第1の含浸部
32 第1の非含浸部
4 第2の樹脂層
41 第2の含浸部
42 第2の非含浸部
10 基板
11 積層体
12 金属層
13 繊維基材
20 界面
100 半導体装置
200 多層基板
201a、201b、201d、201e 回路部
202、203 導体部
300 パッド部
400 配線部
500 半導体素子
501 バンプ
a1、ta2、tb1、tb2 平均厚さ
T 最大厚さ
DESCRIPTION OF SYMBOLS 1, 1a, 1b, 1c, 1d, 1f, 1f Prepreg 2 Fiber base material 3 1st resin layer 31 1st impregnation part 32 1st non-impregnation part 4 2nd resin layer 41 2nd impregnation part 42 Second non-impregnated portion 10 Substrate 11 Laminate 12 Metal layer 13 Fiber base material 20 Interface 100 Semiconductor device 200 Multilayer substrate 201a, 201b, 201d, 201e Circuit portion 202, 203 Conductor portion 300 Pad portion 400 Wiring portion 500 Semiconductor element 501 Bumps t a1 , t a2 , t b1 , t b2 average thickness T maximum thickness

Claims (9)

平板状の繊維基材と、
前記繊維基材の一方の面側に位置し、第1の樹脂組成物で構成された第1の樹脂層と、
前記繊維基材の他方の面側に位置し、前記第1の樹脂組成物と異なる組成の第2の樹脂組成物で構成された第2の樹脂層とを備え、
前記第1の樹脂層は、前記繊維基材の厚さ方向の一部に前記第1の樹脂組成物が含浸した第1の含浸部を有し、
前記第2の樹脂層は、前記第1の樹脂層よりも可撓性が高いものであり、前記繊維基材の前記第1の樹脂組成物が含浸されていない残りの部分に前記第2の樹脂組成物が含浸した第2の含浸部を有し、
前記繊維基材内において、前記第1の含浸部と前記第2の含浸部とが接触しており、
前記第1の含浸部の平均厚さをt a1 [μm]とし、前記第2の含浸部の平均厚さをt b1 [μm]としたとき、t a1 >t b1 なる関係を満足することを特徴とするプリプレグ。
A flat fiber substrate;
A first resin layer located on one side of the fiber substrate and composed of a first resin composition;
A second resin layer that is located on the other surface side of the fiber base material and is composed of a second resin composition having a composition different from that of the first resin composition;
The first resin layer has a first impregnation portion impregnated with the first resin composition in a part of the fiber base in the thickness direction;
The second resin layer is more flexible than the first resin layer, and the second resin layer is not impregnated with the first resin composition , and the second resin layer is not impregnated with the second resin layer. A second impregnation portion impregnated with the resin composition;
In the fiber substrate, the first impregnation part and the second impregnation part are in contact with each other,
When the average thickness of the first impregnated portion is t a1 [μm] and the average thickness of the second impregnated portion is t b1 [μm], the relationship t a1 > t b1 is satisfied. Characteristic prepreg.
前記第1の含浸部と前記第2の含浸部との界面は、凹凸をなす請求項1に記載のプリプレグ。   The prepreg according to claim 1, wherein an interface between the first impregnation part and the second impregnation part is uneven. 前記第2の樹脂層は、前記第1の樹脂層よりも可撓性が高いものであり、
前記第1の樹脂層の前記第1の含浸部を除く部分の平均厚さをta2[μm]とし、前記第2の樹脂層の前記第2の含浸部を除く部分の平均厚さをtb2[μm]としたとき、1.2×ta2<tb2なる関係を満足する請求項1または2に記載のプリプレグ。
The second resin layer is more flexible than the first resin layer,
The average thickness of the portion of the first resin layer excluding the first impregnation portion is t a2 [μm], and the average thickness of the portion of the second resin layer excluding the second impregnation portion is t 3. The prepreg according to claim 1, wherein a relation of 1.2 × t a2 <t b2 is satisfied when b2 [μm] is satisfied.
前記第1の樹脂組成物および前記第2の樹脂組成物は、それぞれ、硬化性樹脂を含み、該硬化性樹脂の種類、含有量、分子量のうちの少なくとも1つが異なるものである請求項1ないし3のいずれかに記載のプリプレグ。 The first resin composition and the second resin composition, respectively, comprising a curable resin, the kind of the curable resin, the content, to at least one of claims 1 to different ones of the molecular weight The prepreg according to any one of 3 above. 前記繊維基材は、ガラス繊維基材である請求項1ないし4のいずれかに記載のプリプレグ。 The prepreg according to any one of claims 1 to 4 , wherein the fiber base material is a glass fiber base material. 請求項1ないし5のいずれかに記載のプリプレグを複数積層してなる積層体を備えることを特徴とする基板。 A substrate comprising a laminate formed by laminating a plurality of the prepregs according to claim 1 . 隣接する前記プリプレグの間に繊維基材をさらに備える請求項6に記載の基板。 The substrate according to claim 6 , further comprising a fiber base material between the adjacent prepregs. 前記積層体の少なくとも一方の面に金属層をさらに備える請求項6または7に記載の基板。 The substrate according to claim 6 or 7 , further comprising a metal layer on at least one surface of the laminate. 請求項6ないし8のいずれかに記載の基板と、
前記基板に搭載された半導体素子とを備えることを特徴とする半導体装置。
A substrate according to any one of claims 6 to 8 ,
A semiconductor device comprising: a semiconductor element mounted on the substrate.
JP2010194260A 2010-08-31 2010-08-31 Prepreg, substrate and semiconductor device Active JP5552969B2 (en)