JP3836164B2 - Barrier packaging material and method for producing the same - Google Patents

Barrier packaging material and method for producing the same Download PDF

Info

Publication number
JP3836164B2
JP3836164B2 JP09841594A JP9841594A JP3836164B2 JP 3836164 B2 JP3836164 B2 JP 3836164B2 JP 09841594 A JP09841594 A JP 09841594A JP 9841594 A JP9841594 A JP 9841594A JP 3836164 B2 JP3836164 B2 JP 3836164B2
Authority
JP
Japan
Prior art keywords
film
barrier
ethylene
layer
packaging material
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP09841594A
Other languages
Japanese (ja)
Other versions
JPH07304139A (en
Inventor
友治 佐藤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toppan Inc
Original Assignee
Toppan Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toppan Inc filed Critical Toppan Inc
Priority to JP09841594A priority Critical patent/JP3836164B2/en
Publication of JPH07304139A publication Critical patent/JPH07304139A/en
Application granted granted Critical
Publication of JP3836164B2 publication Critical patent/JP3836164B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

【0001】
【産業上の利用分野】
本発明は、ガスバリヤー性に優れた包装材料およびその製造方法に関する。
【0002】
【従来の技術】
従来、水蒸気バリヤー性や酸素バリヤー性などの、ガスバリヤー性に優れた包装材料(以下、バリヤー性包装材料という)として、金属箔を含む積層体や金属の蒸着層を形成したプラスチックフィルムを含む積層体が、広く使用されており、袋状の容器に成形(製袋)されて使用されている。そして、上記金属としてはアルミニウムが性能、コスト、加工性の点から一般的に使用されている。
【0003】
ところが、上記金属箔や金属蒸着層はガスバリヤー性を発揮する厚さとした場合には不透明となり、包装材料として使用した際に内容物が透視できないという欠点があった。また、金属箔は、焼却したときに炉の中で塊となってしまい、廃棄性に問題があった。
【0004】
これに対し、エチレン−ビニルアルコール共重合体やポリ塩化ビニリデン等の樹脂層は上記問題がなく、ガスバリヤー性についても、金属層に比べればやや劣るものの十分にバリヤー性材料として実用できるため、バリヤー性包装材料の構成中に一般的に使用されている。さらに、エチレン−ビニルアルコール共重合体は香気成分を透過させない、保香性材料としても知られている。
【0005】
このエチレン−ビニルアルコール共重合体は、例えば厚さ12〜30μmのフィルムとして提供されており、接着剤を用いたドライラミネート、あるいは溶融した熱接着性樹脂の層を介するサンドラミネートにより、他のフィルム(例えば基材フィルムやシーラントフィルム)と積層され、包装材料の一部を構成するのが一般的である。
【0006】
また、ポリ塩化ビニリデンは、上記エチレン−ビニルアルコール共重合体と同様にフィルム状でも使用され、また、適当な溶媒に溶解された溶液を基材フィルムにコーティングして薄い層とし、バリヤー層を形成することもある。
【0007】
【発明が解決しようとする課題】
ところが、上記ポリ塩化ビニリデンは、成分中に塩素を含むため、使用後廃棄する際、焼却すると塩素ガスを発生する。近年は環境保護が叫ばれ、このような樹脂の使用は敬遠されつつある。
【0008】
また、エチレン−ビニルアルコール共重合体は塩素を含まないので環境問題は生じないが、前述のようにフィルム状態で使用されることが一般的であるため、包装材料とするにはドライラミネートなどの積層工程が必須となる。また、材料がフィルム状態で供給されるため厚さの下限があり、通常は12μmが下限である。そして、エチレン−ビニルアルコール共重合体樹脂自体が高価であり、結果として包装材料が高価なものになってしまう。
【0009】
そしてまた、包装材料のガスバリヤー性は、一定範囲内ではこれらの樹脂の厚さに比例するので、要求されるガスバリヤー性によっては、エチレン−ビニルアルコール共重合体フィルムの使用はオーバースペックであり、コスト高でもあり、不経済であった。
【0010】
そこで本発明は、適度な(過度には高くない)ガスバリヤー性を有し、しかもコスト的に優れたバリヤー性包装材料、およびその製造方法を提供するものである。
【0011】
【課題を解決するための手段】
【0012】
発明のバリヤー性包装材料の製造方法の第1は、基材フィルム上に、厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層を含むバリヤーフィルムを共押し出しラミネートし、該バリヤーフィルム上にシーラントフィルムを押し出しラミネートすることを特徴とする、バリヤー性包装材料の製造方法である。
【0013】
また、本発明のバリヤー性包装材料の製造方法の第2は、基材フィルムとシーラントフィルムとの間に、厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層を含むバリヤーフィルムを共押し出しして、前記基材フィルムとシーラントフィルムとをサンドラミネートすることを特徴とする、バリヤー性包装材料の製造方法である。
【0014】
本発明のバリヤー性包装材料およびその製造方法においては、その構成中にポリ塩化ビニリデン層を含まないことが、本発明の目的から好ましい。
また、基材フィルムは延伸フィルムであることが好ましく、印刷層を形成する場合には、前記基材フィルムのバリヤーフィルムが積層される面に形成することが好ましい。
【0015】
【作用】
上記した構成からなる本発明の包装材料は、共押し出しフィルムからなるバリヤーフィルム中に厚さ3〜12μm、好ましくは5〜10μmのエチレン−ビニルアルコール共重合体層をガスバリヤー層として含む。従って、包装材料に一定のガスバリヤー性および香気成分のバリヤー性を付与でき、また、高価なエチレン−ビニルアルコール共重合体樹脂の使用量を小さくすることができるので、全体のコストを抑えることができる。
【0016】
また、本発明のバリヤー性包装材料の製造方法によれば、バリヤーフィルムを共押し出しして、溶融状態にあるうち(すなわち熱接着性が発揮されている間)に基材フィルムに積層するので、バリヤーフィルムを積層する別途の工程が不要となり、包装材料の製造コストを抑えることができる。
【0017】
また、基材フィルムを延伸フィルムとし、該基材フィルムのバリヤーフィルムが積層される面に印刷層を形成することにより、印刷層が保護され、食品等の包装に適した包装材料となる。さらに、平滑な延伸フィルム面に印刷層を形成することになるので、印刷が美麗になる。
【0018】
【実施例】
次に、図面を参照して本発明の実施例を説明する。図1は本発明の包装材料の一実施例を示す断面図、図2は本発明の包装材料の他の実施例を示す断面図である。
【0019】
本発明のバリヤー性包装材料は、図1、図2に示すように、基材フィルム1、バリヤーフィルム2、シーラントフィルム3が順次積層された包装材料であって、前記バリヤーフィルム2が、厚さ3〜12μm、好ましくは5〜10μmのエチレン−ビニルアルコール共重合体層4を含む共押し出しフィルムである。
【0020】
基材フィルム1は、包装材料の主たる層であり、包装材料に機械的強度、テアー性、スリップ性、耐熱性という性質を与える。好ましい材料としては、ポリエチレンテレフタレート、ポリブチレンテレフタレート、ポリエチレンナフタレート等のポリエステルフィルム、6−ナイロン;6,6−ナイロン等のポリアミドフィルム、あるいはポリプロピレンフィルム等の、機械的強度に優れた材料が使用できる。特に、これらの1軸または2軸延伸フィルムを使用することが好ましい。また、これらのフィルムには、必要に応じて周知の添加剤;例えば静電防止剤やスリップ剤、防曇剤、紫外線吸収剤等を添加することができる。また、必要に応じて周知の処理;例えばコロナ放電処理やオゾン処理、フレーム処理等を施すことができる。
【0021】
この基材フィルム1の厚さは特に制限はないが、12〜40μmとすることが好ましい。
【0022】
包装材料には通常印刷層5が形成されるが、図示のように、基材フィルム1のバリヤーフィルム2が積層される面に形成することが好ましい。
【0023】
印刷層5は、通常の方法、すなわちグラビア印刷法、シルクスクリーン印刷法、その他の周知の方法により形成することができる。
【0024】
また、基材フィルム1には、必要に応じて、図示しない介在層や外側層を形成してもよい。例えば、基材フィルム1の外面側または内面側に、風合いの付与や剛度付与の目的のために紙または不織布(坪量15〜90g/m2 )を積層することができる。
【0025】
上記基材フィルム1には、バリヤーフィルム2を積層する。バリヤーフィルム2は、エチレン−ビニルアルコール共重合体の層4を含む共押し出しフィルムである。具体的には、接着性樹脂層6/エチレン−ビニルアルコール共重合体層4/接着性樹脂層6という構成(図1参照)、あるいはエチレン−ビニルアルコール共重合体層4/接着性樹脂層6/ポリオレフィン層7の構成(図2参照)が例示できる。上記バリヤーフィルム2において、エチレン−ビニルアルコール共重合体層4の厚さは、本発明の目的から3〜12μm、好ましくは5〜10μmとする。
【0026】
上記範囲より厚い場合はエチレン−ビニルアルコール共重合体フィルムを用いた場合と比べて樹脂の使用量に差がなく、不経済であり、また、ガスバリヤー性も過剰な場合がある。他方、上記範囲より薄い場合は樹脂の使用量が少ないので好ましいが、連続した均一な層を得ることが困難であり、目的とするガスバリヤー性が得られなくなる恐れがある。
【0027】
また、接着性樹脂層6としては、エチレン−ビニルアルコール共重合体層4との共押し出しが可能で、かつ、隣接することとなる基材フィルム1および/またはシーラントフィルム3あるいはポリオレフィン層7との接着が良好な、ポリエチレン系接着性樹脂(商品名:ADMER NF550、MODIC XM−400M等)やポリプロピレン接着性樹脂(商品名:ADMER QF500等)が採用できる。特に、シーラントフィルム3として無延伸ポリプロピレンを採用するときは、接着性樹脂層6としては上記ポリプロピレン接着性樹脂を採用することが好ましい。この層6の厚さは3〜10μmとすることが好ましい。
【0028】
また、バリヤーフィルム2のポリオレフィン層7(図2参照)としては、エチレン−ビニルアルコール共重合体層4との共押し出し適性およびシーラントフィルム3との接着性を考慮して、低密度ポリエチレン、線状低密度ポリエチレンとすることが好ましい。このポリオレフィン層7の厚さは10〜30μmとすることが好ましい。
【0029】
このバリヤーフィルム2の各層にも、必要に応じて周知の添加剤;例えば静電防止剤やスリップ剤、防曇剤等を添加することができる。また、必要に応じて周知の処理;例えばコロナ放電処理やオゾン処理、フレーム処理等を施すことができる。特に、後述するように本発明においてはバリヤーフィルム2(共押し出しフィルム)を押し出しラミネートないしはサンドラミネートすることにより積層するので、基材フィルム1やバリヤーフィルム2、あるいはシーラントフィルム3に使用する樹脂の種類によっては、バリヤーフィルム2に対するコロナ放電処理やオゾン処理等の接着性改善処理が必須となる。
【0030】
このバリヤーフィルム2の全体的な厚さは特に制限はないが、共押し出しの性質上、10〜50μmの範囲が一般的である。
【0031】
次に、シーラントフィルム3は、包装材料にヒートシール性を付与する層であり、通常使用されている材料が使用できる。
具体的には、低密度ポリエチレン、線状低密度ポリエチレン、エチレン−酢酸ビニル共重合体、無延伸ポリプロピレン、アイオノマー、エチレン−アクリル酸共重合体(EAA)、エチレン−メタクリル酸共重合体(EMAA)等の樹脂が使用できる。また、特殊な用途;例えば保香性を目的とする場合においては、ヒートシール性ポリエステルやエチレン−ビニルアルコール共重合体などのヒートシール性樹脂も使用され得る。後述のように、この層は、押し出しラミネートによりバリヤーフィルム2の上に直接形成してもよく、あるいはフィルム状態のものをラミネートしてもよい。また、前述した共押し出しによるバリヤーフィルムの製造の際、シーラントフィルム3を同時に共押し出しし、一体化するようにしてもよい。
【0032】
このシーラントフィルム3の厚さは、10〜100μm、特に20〜80μmとすることが好ましい。
【0033】
以上の各層は、押し出しラミネート、またはバリヤーフィルム2を接着層として用いるサンドラミネートにより積層される。
【0034】
図1に示した実施例は、基材フィルム1上にバリヤーフィルム2を共押し出しラミネートし、該バリヤーフィルム2上にシーラントフィルム3を押し出しラミネートして得たものである。また、図2に示した実施例は、基材フィルム1とシーラントフィルム3とを準備し、この両者の間に、バリヤーフィルム2を共押し出しして、前記基材フィルム1とシーラントフィルム3とをサンドラミネートして得たものである。なお、これらのラミネートに先立ち、積層面にアンカーコーティング剤をコートしたり、前述したとおりの前処理(コロナ処理やオゾン処理等)を、必要に応じて行うことができる。
【0035】
上述のように押し出しラミネートまたはサンドラミネートを適用することにより、従来広く行われているドライラミネートといった、各層の接着のみを目的とする工程が省略でき、従って包装材料全体のコストを下げることができるので好ましい。
【0036】
上述した本発明による包装材料の具体的構成例を以下に列挙する。なお、下記において "EX" は押し出しラミネートによる層を示し、 " [ ] " 内の層は共押し出しによる層を示す。また、右肩の数字は厚さ(μm)である。
【0037】
(1) AS-OPP30/印/AC/[EVOH5/接5/PE15]/EX-AS-EVA25
(2) AS-OPP30/印/AC/[接5/EVOH5/接5]/AS-EVA40
(3) OPP20/印/AC/[EVOH5/接3/PE20]/EX-EVA30
(4) OPP25/印/AC/[EVOH10/接5/PE20]/EX-EVA30
(5) OPP25/印/AC/[EVOH10/接5/CPP30]
(6) OPP20/印/AC/[接5/EVOH5/接5]/CPP40
(7) PET12/印/AC/[EVOH5/接5/LLDPE20]/EX-LLDPE30
(8) PET12/印/AC/[接5/EVOH5/接5]/CPP40
(9) NY15/印/AC/[EVOH5/接5/PE20]/EX-LLDPE30
(10)NY15/印/AC/[接5/EVOH5/接5]/LLDPE50
PE:低密度ポリエチレン
LLDPE:線状低密度ポリエチレン
EVA:エチレン−酢酸ビニル共重合体
CPP:無延伸ポリプロピレン
OPP:2軸延伸ポリプロピレン
PET:2軸延伸ポリエチレンテレフタレート
NY:延伸6−ナイロン
EVOH:エチレン−ビニルアルコール共重合体層
接:接着性樹脂層
印:印刷層
AC:アンカーコート層
AS−:静電防止剤練り込み
【0038】
上記(1)(3)(4)(5)(7)(9)はバリヤーフィルムを押し出しラミネートにより積層し たものである。また、(2)(6)(8)(10) はバリヤーフィルム(共押し出しフィルム)を間に挟んだサンドラミネートにより積層して得たものである。なお、▲5▼はシーラントフィルム3(CPP)をバリヤーフィルム2の製造時に同時に共押し出ししたものである。
【0039】
以上のようにして得られた本発明の包装材料は、一般的にはシーラントフィルム3同士をヒートシールして、3方ないしは4方シール袋、ガゼット袋、スタンディングパウチ、ピロー包装袋等として使用される。また、本発明の包装材料を適宜形状に打ち抜き、容器のヒートシール蓋として使用することもできる。また、本発明の包装材料をチューブ容器の胴部材として使用することもできる。
【0040】
そして、本発明の包装材料は酸素透過度が0.3〜2.0cc/m2 ・24hrs ・atm 、水蒸気透過度が2〜10g/m2 ・24hrs というバリヤー性を示す。従って、本発明の包装材料は、酸化による変褪色や変味、微生物の繁殖による腐敗、黴の発生等の防止、さらには保香性等が要求される、削り節、漬物、佃煮、スナック菓子、豆菓子、カステラ、饅頭、味噌、乾麺、ペットフード、ハム・ソーセージ、バター、チーズ、餅等の食品類の包装に適している。
【0041】
<実施例1>
厚さ30μmの2軸延伸ポリプロピレンフィルムに、ポリウレタン系樹脂をビヒクルとするインキで印刷層を形成した。この印刷層上に、ポリウレタン系樹脂を主成分とするアンカーコート剤を9g/m2 の塗布量で塗布した。この上に、3種3層共押し出し機により、エチレン−ビニルアルコール共重合体層(10μm)/接着性樹脂層(ポリエチレン系;MODIC XM−400M:5μm)/低密度ポリエチレン(20μm)の構成の共押し出しフィルム(バリヤーフィルム)を押し出しラミネートした。さらに、上記低密度ポリエチレン上に、厚さ30μmの線状低密度ポリエチレン(シーラントフィルム)を押し出しラミネートにより積層し、本発明のバリヤー性包装材料を得た。
【0042】
得られた包装材料のバリヤー性を測定したところ、酸素透過度は0.5cc/m2 ・24hrs ・atm 、水蒸気透過度は4g/m2 ・24hrs であった。
また、印刷は非常に美麗であった。
【0043】
<実施例2>
厚さ30μmの2軸延伸ポリプロピレンフィルムに、ポリウレタン系樹脂をビヒクルとするインキで印刷層を形成した。この印刷層上に、ポリウレタン系樹脂を主成分とするアンカーコート剤を4g/m2 の塗布量で塗布した。この2軸延伸ポリプロピレンフィルムの印刷層面と、厚さ30μmの線状低密度ポリエチレン(シーラントフィルム)との間に、3種3層共押し出し機により、接着性樹脂層(ポリエチレン系;MODIC XM−400M:5μm)/エチレン−ビニルアルコール共重合体層(10μm)/接着性樹脂層(ポリエチレン系;MODIC XM−400M:5μm)の構成の共押し出しフィルム(バリヤーフィルム)を押し出してサンドラミネートにより積層し、本発明のバリヤー性包装材料を得た。
【0044】
得られた包装材料のバリヤー性を測定したところ、酸素透過度は0.5cc/m2 ・24hrs ・atm 、水蒸気透過度は4g/m2 ・24hrs であった。
【0045】
【発明の効果】
以上述べたように、本発明のバリヤー性包装材料は、高価なエチレン−ビニルアルコール共重合体を共押し出しフィルムとしたので、該層を薄くでき、コストを抑えることができる。また、本発明の製造方法によれば、単なる積層のための工程を省略でき、製造コストを抑えることができる。
【0046】
そして、本発明によれば、バリヤー層としてのエチレン−ビニルアルコール共重合体層の厚さを任意の厚さに容易に変更ができ、ガスバリヤー性を任意に調整することができる。
【0047】
また、得られた包装材料は、適度なガスバリヤー性と保香性を有するので、これまでポリ塩化ビニリデンのコーティング層をバリヤー層として有していた包装材料の、環境保護可能な代替材料として使用することができる。また、本発明の包装材料は、これまでエチレン−ビニルアルコール共重合体フィルムをバリヤー層として有していたためにガスバリヤー性が高すぎていた材料に代えて、適度なガスバリヤー性を有する代替材料として使用することができる。
【0048】
そして、印刷層を基材フィルムの内面(裏面)側に形成した場合は、優れた印刷効果、美麗性を有するものとなる。
【図面の簡単な説明】
【図1】本発明の包装材料の一実施例を示す断面図である。
【図2】本発明の包装材料の他の実施例を示す断面図である。
【符号の説明】
1……基材フィルム
2……バリヤーフィルム
3……シーラントフィルム
4……エチレン−ビニルアルコール共重合体
5……印刷層
6……接着性樹脂
7……ポリオレフィン
[0001]
[Industrial application fields]
The present invention relates to a packaging material excellent in gas barrier properties and a method for producing the same.
[0002]
[Prior art]
Conventionally, as a packaging material excellent in gas barrier properties such as water vapor barrier property and oxygen barrier property (hereinafter referred to as barrier packaging material), a laminate including a laminate including a metal foil or a plastic film having a metal vapor-deposited layer formed thereon. The body is widely used, and is molded (made into a bag) into a bag-like container. And as said metal, aluminum is generally used from the point of performance, cost, and workability.
[0003]
However, the metal foil and the metal vapor-deposited layer are opaque when the thickness exhibits gas barrier properties, and the contents cannot be seen through when used as a packaging material. In addition, when the metal foil is incinerated, it becomes a lump in the furnace, and there is a problem in discardability.
[0004]
On the other hand, resin layers such as ethylene-vinyl alcohol copolymer and polyvinylidene chloride do not have the above-mentioned problems, and the gas barrier property is slightly inferior to that of the metal layer, but can be practically used as a barrier material. Commonly used in the construction of adhesive packaging materials. Furthermore, the ethylene-vinyl alcohol copolymer is also known as an aroma retaining material that does not allow permeation of aroma components.
[0005]
This ethylene-vinyl alcohol copolymer is provided, for example, as a film having a thickness of 12 to 30 μm, and other films can be obtained by dry lamination using an adhesive or by sand lamination via a molten layer of a heat-adhesive resin. It is generally laminated with (for example, a base film or a sealant film) to constitute a part of the packaging material.
[0006]
Polyvinylidene chloride is also used in the same film form as the ethylene-vinyl alcohol copolymer, and a thin film is formed by coating a base film with a solution dissolved in an appropriate solvent to form a barrier layer. Sometimes.
[0007]
[Problems to be solved by the invention]
However, since the polyvinylidene chloride contains chlorine in its components, chlorine gas is generated when incinerated when discarded after use. In recent years, environmental protection has been screamed, and the use of such resins is being avoided.
[0008]
In addition, since ethylene-vinyl alcohol copolymer does not contain chlorine, it does not cause environmental problems. However, since it is generally used in a film state as described above, a dry laminate or the like is used as a packaging material. A lamination process is essential. Further, since the material is supplied in a film state, there is a lower limit of the thickness, and usually 12 μm is the lower limit. And ethylene-vinyl alcohol copolymer resin itself is expensive, and as a result, the packaging material becomes expensive.
[0009]
In addition, since the gas barrier property of the packaging material is proportional to the thickness of these resins within a certain range, depending on the required gas barrier property, the use of the ethylene-vinyl alcohol copolymer film is overspec. It was expensive and uneconomical.
[0010]
Therefore, the present invention provides a barrier packaging material having an appropriate (not excessively high) gas barrier property and excellent in cost, and a method for producing the same.
[0011]
[Means for Solving the Problems]
[0012]
A first method for producing a barrier packaging material according to the present invention is a method of coextruding a barrier film containing an ethylene-vinyl alcohol copolymer layer having a thickness of 3 to 12 μm on a base film and laminating the barrier film on the barrier film. A method for producing a barrier packaging material, wherein a sealant film is extruded and laminated .
[0013]
In the second method for producing a barrier packaging material of the present invention, a barrier film containing an ethylene-vinyl alcohol copolymer layer having a thickness of 3 to 12 μm is coextruded between a base film and a sealant film. A method for producing a barrier packaging material , wherein the substrate film and the sealant film are sand-laminated .
[0014]
In the barrier packaging material and the method for producing the same of the present invention, it is preferable from the object of the present invention that the polyvinylidene chloride layer is not included in the constitution.
Moreover, it is preferable that a base film is a stretched film, and when forming a printing layer, it is preferable to form in the surface where the barrier film of the said base film is laminated | stacked.
[0015]
[Action]
The packaging material of the present invention having the above-described configuration includes an ethylene-vinyl alcohol copolymer layer having a thickness of 3 to 12 μm, preferably 5 to 10 μm, as a gas barrier layer in a barrier film made of a coextruded film. Therefore, it is possible to impart a certain gas barrier property and fragrance component barrier property to the packaging material, and to reduce the amount of expensive ethylene-vinyl alcohol copolymer resin used, thereby reducing the overall cost. it can.
[0016]
Further, according to the method for producing a barrier packaging material of the present invention, the barrier film is coextruded and laminated on the base film while it is in a molten state (that is, while thermal adhesiveness is exerted) A separate process for laminating the barrier film becomes unnecessary, and the manufacturing cost of the packaging material can be reduced.
[0017]
In addition, by forming a base film as a stretched film and forming a print layer on the surface of the base film on which the barrier film is laminated, the print layer is protected and a packaging material suitable for packaging foods and the like is obtained. Further, since the printing layer is formed on the smooth stretched film surface, the printing becomes beautiful.
[0018]
【Example】
Next, embodiments of the present invention will be described with reference to the drawings. FIG. 1 is a sectional view showing an embodiment of the packaging material of the present invention, and FIG. 2 is a sectional view showing another embodiment of the packaging material of the present invention.
[0019]
As shown in FIGS. 1 and 2, the barrier packaging material of the present invention is a packaging material in which a base film 1, a barrier film 2, and a sealant film 3 are sequentially laminated, and the barrier film 2 has a thickness. A coextruded film comprising an ethylene-vinyl alcohol copolymer layer 4 of 3 to 12 μm, preferably 5 to 10 μm.
[0020]
The base film 1 is a main layer of the packaging material, and gives the packaging material properties such as mechanical strength, tear properties, slip properties, and heat resistance. As a preferable material, a material excellent in mechanical strength such as a polyester film such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, 6-nylon; a polyamide film such as 6,6-nylon, or a polypropylene film can be used. . In particular, it is preferable to use these uniaxially or biaxially stretched films. Moreover, well-known additives; for example, an antistatic agent, a slip agent, an antifogging agent, an ultraviolet absorber, etc. can be added to these films as needed. Moreover, a well-known process; for example, a corona discharge process, an ozone process, a flame process etc. can be performed as needed.
[0021]
The thickness of the base film 1 is not particularly limited, but is preferably 12 to 40 μm.
[0022]
The printing material 5 is usually formed on the packaging material, but it is preferably formed on the surface of the base film 1 on which the barrier film 2 is laminated, as shown.
[0023]
The printing layer 5 can be formed by a normal method, that is, a gravure printing method, a silk screen printing method, or other known methods.
[0024]
Moreover, you may form the intervening layer and outer layer which are not shown in figure in the base film 1 as needed. For example, paper or a nonwoven fabric (basis weight 15-90 g / m < 2 >) can be laminated | stacked on the outer surface side or inner surface side of the base film 1 for the purpose of provision of a texture or rigidity.
[0025]
A barrier film 2 is laminated on the base film 1. The barrier film 2 is a coextruded film comprising a layer 4 of ethylene-vinyl alcohol copolymer. Specifically, the configuration of adhesive resin layer 6 / ethylene-vinyl alcohol copolymer layer 4 / adhesive resin layer 6 (see FIG. 1), or ethylene-vinyl alcohol copolymer layer 4 / adhesive resin layer 6 / The configuration of the polyolefin layer 7 (see FIG. 2) can be exemplified. In the barrier film 2, the thickness of the ethylene-vinyl alcohol copolymer layer 4 is 3 to 12 μm, preferably 5 to 10 μm for the purpose of the present invention.
[0026]
When the thickness is larger than the above range, there is no difference in the amount of resin used compared to the case of using an ethylene-vinyl alcohol copolymer film, which is uneconomical and may have an excessive gas barrier property. On the other hand, when the thickness is smaller than the above range, it is preferable because the amount of the resin used is small, but it is difficult to obtain a continuous and uniform layer, and the target gas barrier property may not be obtained.
[0027]
The adhesive resin layer 6 can be co-extruded with the ethylene-vinyl alcohol copolymer layer 4 and is adjacent to the base film 1 and / or the sealant film 3 or the polyolefin layer 7. A polyethylene-based adhesive resin (trade name: ADMER NF550, MODIC XM-400M, etc.) or a polypropylene adhesive resin (trade name: ADMER QF500, etc.) having good adhesion can be used. In particular, when unstretched polypropylene is employed as the sealant film 3, it is preferable to employ the polypropylene adhesive resin as the adhesive resin layer 6. The thickness of this layer 6 is preferably 3 to 10 μm.
[0028]
The polyolefin film 7 of the barrier film 2 (see FIG. 2) is a low-density polyethylene, linear, considering coextrusion suitability with the ethylene-vinyl alcohol copolymer layer 4 and adhesiveness with the sealant film 3. Low density polyethylene is preferred. The thickness of the polyolefin layer 7 is preferably 10 to 30 μm.
[0029]
A known additive; for example, an antistatic agent, a slip agent, an antifogging agent, or the like can be added to each layer of the barrier film 2 as necessary. Moreover, a well-known process; for example, a corona discharge process, an ozone process, a flame process etc. can be performed as needed. In particular, since the barrier film 2 (coextruded film) is laminated by extrusion lamination or sand lamination in the present invention as will be described later, the kind of resin used for the base film 1, the barrier film 2, or the sealant film 3 Depending on the case, the barrier film 2 must be subjected to an adhesive improvement treatment such as corona discharge treatment or ozone treatment.
[0030]
The overall thickness of the barrier film 2 is not particularly limited, but is generally in the range of 10 to 50 μm because of the coextrusion property.
[0031]
Next, the sealant film 3 is a layer that imparts heat sealability to the packaging material, and a commonly used material can be used.
Specifically, low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, unstretched polypropylene, ionomer, ethylene-acrylic acid copolymer (EAA), ethylene-methacrylic acid copolymer (EMAA) Etc. can be used. In addition, for special purposes; for example, in the case of aroma retention, a heat-sealable resin such as a heat-sealable polyester or an ethylene-vinyl alcohol copolymer may also be used. As will be described later, this layer may be formed directly on the barrier film 2 by extrusion lamination, or may be laminated in a film state. Further, when the barrier film is manufactured by the co-extrusion described above, the sealant film 3 may be co-extruded at the same time and integrated.
[0032]
The thickness of the sealant film 3 is preferably 10 to 100 μm, more preferably 20 to 80 μm.
[0033]
Each of the above layers is laminated by extrusion lamination or sand lamination using the barrier film 2 as an adhesive layer.
[0034]
The example shown in FIG. 1 is obtained by coextrusion laminating a barrier film 2 on a base film 1 and extruding and laminating a sealant film 3 on the barrier film 2. In the embodiment shown in FIG. 2, a base film 1 and a sealant film 3 are prepared, and the barrier film 2 is coextruded between the two, whereby the base film 1 and the sealant film 3 are combined. It was obtained by sand lamination. Prior to these laminations, the laminated surface can be coated with an anchor coating agent, or pretreatment as described above (corona treatment, ozone treatment, etc.) can be performed as necessary.
[0035]
By applying an extrusion laminate or a sand laminate as described above, it is possible to omit a process only for bonding each layer, such as a dry laminate, which has been widely performed in the past, and thus the cost of the entire packaging material can be reduced. preferable.
[0036]
Specific configuration examples of the packaging material according to the present invention described above are listed below. In the following, “EX” indicates a layer formed by extrusion lamination, and a layer in “[]” indicates a layer formed by co-extrusion. The number on the right shoulder is the thickness (μm).
[0037]
(1) AS-OPP 30 / mark / AC / [EVOH 5 / contact 5 / PE 15 ] / EX-AS-EVA 25
(2) AS-OPP 30 / indicia / AC / [contact 5 / EVOH 5 / contact 5] / AS-EVA 40
(3) OPP 20 / mark / AC / [EVOH 5 / contact 3 / PE 20 ] / EX-EVA 30
(4) OPP 25 / mark / AC / [EVOH 10 / contact 5 / PE 20 ] / EX-EVA 30
(5) OPP 25 / mark / AC / [EVOH 10 / contact 5 / CPP 30 ]
(6) OPP 20 / indicia / AC / [contact 5 / EVOH 5 / contact 5] / CPP 40
(7) PET 12 / mark / AC / [EVOH 5 / contact 5 / LLDPE 20 ] / EX-LLDPE 30
(8) PET 12 / indicia / AC / [contact 5 / EVOH 5 / contact 5] / CPP 40
(9) NY 15 / mark / AC / [EVOH 5 / contact 5 / PE 20 ] / EX-LLDPE 30
(10) NY 15 / indicia / AC / [contact 5 / EVOH 5 / contact 5] / LLDPE 50
PE: low density polyethylene LLDPE: linear low density polyethylene EVA: ethylene-vinyl acetate copolymer CPP: unstretched polypropylene OPP: biaxially stretched polypropylene PET: biaxially stretched polyethylene terephthalate NY: stretched 6-nylon EVOH: ethylene-vinyl Alcohol copolymer layer contact: adhesive resin layer mark: printed layer AC: anchor coat layer AS-: kneaded antistatic agent
The above (1), (3), (4), (5), (7), and (9) are obtained by laminating barrier films by extrusion lamination. Also, (2), (6), (8), and (10) are obtained by laminating by a sand laminate with a barrier film (coextruded film) sandwiched therebetween. In addition, (5) is obtained by coextruding the sealant film 3 (CPP) at the same time when the barrier film 2 is manufactured.
[0039]
The packaging material of the present invention obtained as described above is generally used as a three- or four-side sealed bag, a gusset bag, a standing pouch, a pillow packaging bag, etc. by heat sealing the sealant films 3 to each other. The Further, the packaging material of the present invention can be appropriately punched into a shape and used as a heat seal lid for a container. Moreover, the packaging material of this invention can also be used as a trunk | drum member of a tube container.
[0040]
The packaging material of the present invention exhibits barrier properties such as an oxygen permeability of 0.3 to 2.0 cc / m 2 · 24 hrs · atm and a water vapor permeability of 2 to 10 g / m 2 · 24 hrs. Therefore, the packaging material of the present invention is required to have a discoloration and taste due to oxidation, spoilage due to the propagation of microorganisms, generation of spider, etc., and further to maintain aroma, etc., shaving, pickles, boiled, snacks, beans It is suitable for packaging foods such as confectionery, castella, buns, miso, dried noodles, pet food, ham / sausage, butter, cheese, and candy.
[0041]
<Example 1>
A printing layer was formed on a biaxially stretched polypropylene film having a thickness of 30 μm with an ink using a polyurethane-based resin as a vehicle. On this printed layer, an anchor coating agent mainly composed of a polyurethane resin was applied at an application amount of 9 g / m 2 . On top of this, the composition of ethylene-vinyl alcohol copolymer layer (10 μm) / adhesive resin layer (polyethylene type; MODIC XM-400M: 5 μm) / low density polyethylene (20 μm) was formed by a three-type three-layer coextrusion machine. A coextruded film (barrier film) was extruded and laminated. Further, a linear low density polyethylene (sealant film) having a thickness of 30 μm was laminated on the low density polyethylene by extrusion lamination to obtain a barrier packaging material of the present invention.
[0042]
When the barrier property of the obtained packaging material was measured, the oxygen permeability was 0.5 cc / m 2 · 24 hrs · atm, and the water vapor permeability was 4 g / m 2 · 24 hrs.
Also, the printing was very beautiful.
[0043]
<Example 2>
A printing layer was formed on a biaxially stretched polypropylene film having a thickness of 30 μm with an ink using a polyurethane-based resin as a vehicle. On this printed layer, an anchor coating agent mainly composed of a polyurethane resin was applied at a coating amount of 4 g / m 2 . An adhesive resin layer (polyethylene-based; MODIC XM-400M) is formed between the printed layer surface of the biaxially oriented polypropylene film and a linear low-density polyethylene (sealant film) having a thickness of 30 μm by a three-type three-layer coextrusion machine. : 5 μm) / ethylene-vinyl alcohol copolymer layer (10 μm) / adhesive resin layer (polyethylene type; MODIC XM-400M: 5 μm), a co-extruded film (barrier film) is extruded and laminated by sand lamination, The barrier packaging material of the present invention was obtained.
[0044]
When the barrier property of the obtained packaging material was measured, the oxygen permeability was 0.5 cc / m 2 · 24 hrs · atm, and the water vapor permeability was 4 g / m 2 · 24 hrs.
[0045]
【The invention's effect】
As described above, since the barrier packaging material of the present invention uses an expensive ethylene-vinyl alcohol copolymer as a coextruded film, the layer can be thinned and the cost can be reduced. Moreover, according to the manufacturing method of this invention, the process for mere lamination | stacking can be abbreviate | omitted and manufacturing cost can be held down.
[0046]
And according to this invention, the thickness of the ethylene-vinyl alcohol copolymer layer as a barrier layer can be easily changed into arbitrary thickness, and gas barrier property can be adjusted arbitrarily.
[0047]
In addition, since the obtained packaging material has appropriate gas barrier properties and fragrance retention properties, it can be used as an environmentally friendly alternative to packaging materials that previously had a polyvinylidene chloride coating layer as a barrier layer. can do. In addition, the packaging material of the present invention is an alternative material having an appropriate gas barrier property instead of a material that has had an ethylene-vinyl alcohol copolymer film as a barrier layer so far that the gas barrier property is too high. Can be used as
[0048]
And when a printing layer is formed in the inner surface (back surface) side of a base film, it has the outstanding printing effect and beauty.
[Brief description of the drawings]
FIG. 1 is a cross-sectional view showing an embodiment of a packaging material of the present invention.
FIG. 2 is a cross-sectional view showing another embodiment of the packaging material of the present invention.
[Explanation of symbols]
DESCRIPTION OF SYMBOLS 1 ... Base film 2 ... Barrier film 3 ... Sealant film 4 ... Ethylene-vinyl alcohol copolymer 5 ... Printing layer 6 ... Adhesive resin 7 ... Polyolefin

Claims (6)

厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層の両面にポリエチレン系接着性樹脂又はポリプロピレン系接着性樹脂を積層したバリヤーフィルムを共押し出しラミネートして、基材フィルム上に積層し、バリヤーフィルムの接着性樹脂層上にシーラントフィルムを押し出しラミネートして積層することを特徴とするバリヤー性包装材料の製造方法。 Thick 3~12μm ethylene - a barrier film obtained by laminating a polyethylene-based adhesive resin or polypropylene based adhesive resin to both surfaces of the vinyl alcohol copolymer layer and laminate-Shi pushed out co, laminated on a base film the method of barrier packaging material characterized by laminating and out Shi laminate-pressing sealant film contacting adhesive resin layer Bas rear film. 厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層ポリエチレン系接着性樹脂又はポリプロピレン系接着性脂層/ポリオレフィン樹脂層の構成であるバリヤーフィルムを、共押し出しラミネートしてエチレン‐ビニルアルコール共重合体層面が基材フィルムに面するように、基材フィルム上に積層し、バリヤーフィルムのポリオレフィン樹脂層上にシーラントフィルムを押し出しラミネートして積層することを特徴とするバリヤー性包装材料の製造方法。 Thick 3~12μm ethylene - a barrier film is the configuration of the vinyl alcohol copolymer layer / polyethylene-based adhesive resin or polypropylene-based adhesive resins layers / polyolefin resin layer, and coextrusion laminating an ethylene - vinyl alcohol copolymer as the polymer layer surface facing the base film, barrier wrap, characterized in that laminated on a base film, laminating and out Shi laminate-pressing sealant film to the polyolefin resin layer Bas rear film Material manufacturing method. 基材フィルムとシーラントフィルムとの間に、厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層の両面にポリエチレン系接着性樹脂又はポリプロピレン系接着性樹脂層を積層したバリヤーフィルムを共押し出しし、基材フィルムとシーラントフィルムとの間にサンドラミネートすることを特徴とするバリヤー性包装材料の製造方法。Between the base film and sealant film, an ethylene thick 3 to 12 [mu] m - Shi pushed out co barrier film obtained by laminating a polyethylene-based adhesive resin or polypropylene based adhesive resin layer on both surfaces of the vinyl alcohol copolymer layer to method for producing a barrier packaging material, characterized in that the sand laminated between the base film and the sealant film. 基材フィルムとシーラントフィルムとの間に、厚さ3〜12μmのエチレン‐ビニルアルコール共重合体層ポリエチレン系接着性樹脂又はポリプロピレン系接着性脂層/ポリオレフィン樹脂層の構成であるバリヤーフィルムを、エチレンビニルアルコール共重合体層面が基材フィルムに面して積層されるように共押し出しし、基材フィルムとシーラントフィルムの間にサンドラミネートすることを特徴とするバリヤー性包装材料の製造方法。Between the base film and sealant film, an ethylene thick 3 to 12 [mu] m - a barrier film is a vinyl alcohol copolymer layer / polyethylene-based adhesive resin or polypropylene-based adhesive resins layers / polyolefin resin layer structure , ethylene - barrier packaging material, characterized in that the sand laminated between the vinyl to be lion pushed out co as alcohol copolymer layer surface is laminated facing the base film, the base film and sealant film Manufacturing method. 請求項1乃至のいずれか1項記載のバリヤー性包装材料の製造方法であって前記基材フィルムが、ポリエチレンテレフタレート、ポリブチレンテレフタレート、ポリエチレンナフタレート等のポリエステルフィルム、6‐ナイロン、6,6‐ナイロン等のポリアミドフィルム、ポリプロピレンフィルムのいずれか1種延伸フィルムであり、該基材フィルムのバリヤーフィルムが積層される面に印刷層を形成することを特徴とするバリヤー性包装材料の製造方法。Claims 1 to said substrate film A method of manufacturing a barrier packaging material according to any one of 4, polyethylene terephthalate, polybutylene terephthalate, polyester film such as polyethylene naphthalate, 6-nylon, 6,6 -A method for producing a barrier packaging material, characterized in that it is a stretched film of any one of a polyamide film such as nylon and a polypropylene film, and a printed layer is formed on the surface of the base film on which the barrier film is laminated. . 請求項1乃至のいずれか1項記載のバリヤー性包装材料の製造方法であって前記シーラントフィルムが、低密度ポリエチレン、線状低密度ポリエチレン、エチレン‐酢酸ビニル共重合体、無延伸ポリプロピレン、アイオノマー、エチレン‐アクリル酸共重合体、エチレン‐メタクリル酸共重合体、ヒートシール性ポリエステル、エチレン‐ビニルアルコール共重合体のいずれか1種の樹脂からなるフィルムであることを特徴とするバリヤー性包装材料の製造方法。The method for producing a barrier packaging material according to any one of claims 1 to 5 , wherein the sealant film is low density polyethylene, linear low density polyethylene, ethylene-vinyl acetate copolymer, unstretched polypropylene, ionomer. A barrier packaging material characterized by being a film made of any one resin of ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, heat- sealable polyester, and ethylene-vinyl alcohol copolymer Manufacturing method.
JP09841594A 1994-05-12 1994-05-12 Barrier packaging material and method for producing the same Expired - Lifetime JP3836164B2 (en)