JP2860716B2 - Grout injection - Google Patents

Grout injection

Info

Publication number
JP2860716B2
JP2860716B2 JP6049291A JP6049291A JP2860716B2 JP 2860716 B2 JP2860716 B2 JP 2860716B2 JP 6049291 A JP6049291 A JP 6049291A JP 6049291 A JP6049291 A JP 6049291A JP 2860716 B2 JP2860716 B2 JP 2860716B2
Authority
JP
Japan
Prior art keywords
blast furnace
seawater
furnace slag
granulated blast
grout
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP6049291A
Other languages
Japanese (ja)
Other versions
JPH04293992A (en
Inventor
伸行 藤澤
正俊 飯尾
智之 関口
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Raito Kogyo Co Ltd
Original Assignee
Raito Kogyo Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Raito Kogyo Co Ltd filed Critical Raito Kogyo Co Ltd
Priority to JP6049291A priority Critical patent/JP2860716B2/en
Publication of JPH04293992A publication Critical patent/JPH04293992A/en
Application granted granted Critical
Publication of JP2860716B2 publication Critical patent/JP2860716B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は、グラウト注入剤に関す
る。
The present invention relates to grout fillers.

【0002】[0002]

【従来の技術】地盤の改良のためのグラウト注入剤とし
ては、種々のものが従来から用いられてきた。現在の多
くは、水ガラス系またはセメント系のものが大半であ
る。
2. Description of the Related Art Various grout fillers have been used for improving the ground. Most of them are currently water glass or cement based.

【0003】我が国のグラウト剤の歴史を振り返ってみ
れば、1960年代に樋口氏がセメント懸濁液と希釈水ガラ
ス溶液とを組み合わせたゲルタイムの短い不安定水ガラ
スグラウト(LW)、その後このLWに改良を加えて、
微粒子の高炉コロイドセメントと低モル比の水ガラス希
釈溶液とを組み合わせた、ゲルタイムが十数分の高強度
で恒久性の高い不安定水ガラスグラウト(C−LW)、
さらに高炉水砕スラグとポルトランドセメントの混合比
率を変化させ各モル比の水ガラス希釈溶液とを組み合わ
せた比較的にゲルタイムの長いグラウト(MS)が基礎
になっている。
[0003] Looking back on the history of grouting agents in Japan, in the 1960s, Higuchi proposed an unstable water glass grout (LW) with a short gel time combining a cement suspension and a diluted water glass solution. With improvements,
An unstable water glass grout (C-LW), which is a combination of a blast furnace colloid cement of fine particles and a low molar ratio water glass diluting solution, has a gel time of more than ten times, and has a high strength and high durability.
Furthermore, grout (MS) having a relatively long gel time based on a change in the mixing ratio of granulated blast furnace slag and Portland cement and combination with a water glass dilute solution at each molar ratio is based.

【0004】現在では、浸透を目的とした場合には、水
ガラスと硬化剤とを組み合わせた溶液型のものが多い。
At present, for the purpose of infiltration, there are many solution types in which water glass and a curing agent are combined.

【0005】しかし、懸濁液型または半懸濁液型のもの
も、高い強度を得るためには、有効であるために、多く
用いられている。
However, a suspension type or a semi-suspension type is also widely used because it is effective for obtaining high strength.

【0006】[0006]

【発明が解決しようとする課題】高炉水砕スラグなどの
カルシウムを含む化合物に対してアルカリを添加する
と、加水分解が生じて高炉水砕スラグの潜在水硬性が発
現する。しかし、この場合、スラグ粒子はアルカリの溶
液と接触すると、スラグ中のSiO2、Al2O3 が溶出し、次
にCa2+イオンが溶出し、これにより、スラグ粒子表面に
ケイ酸カルシウム水和物が生成し、スラグ粒子相互を凝
集結合させる。しかし、アルカリの添加が必要となり、
未反応のアルカリが地盤中に残存し、アルカリの種類に
より地盤を汚染する危険性がある。
When an alkali is added to a compound containing calcium, such as granulated blast furnace slag, hydrolysis occurs, and the latent hydraulic property of the granulated blast furnace slag is developed. However, in this case, when the slag particles come into contact with an alkaline solution, SiO 2 and Al 2 O 3 in the slag elute, and then Ca 2+ ions elute, thereby causing the calcium silicate water to adhere to the slag particle surface. A hydrate is formed, causing the slag particles to cohere. However, the addition of alkali is required,
Unreacted alkali remains in the ground, and there is a risk of soil contamination depending on the type of alkali.

【0007】他方、グラウトの注入に際しては、従来、
専ら清水、通常水道水が用いられている。高炉水砕スラ
グに対して、清水を添加した場合であっても、粒子が微
粒であることによる物理的作用による他、化学的に加水
分解を生じ、ポルトランドセメントと同様に硬化する。
しかし、この場合には、後述のように、ブリージング率
が大きく、かつ地盤に対する浸透性が良好でない。
On the other hand, when grout is injected, conventionally,
Only fresh water, usually tap water, is used. Even when fresh water is added to the granulated blast furnace slag, it is chemically hydrolyzed and hardened in the same manner as Portland cement, in addition to the physical action due to the fine particles.
However, in this case, as described later, the breathing rate is large and the permeability to the ground is not good.

【0008】したがって、本発明の課題は、高炉水砕ス
ラグなどのカルシウム含有物の優れた水硬性をそのまま
利用してグラウト注入剤とする場合において、ブリージ
ング率を低下させ、浸透性の改良を図ることにある。
[0008] Accordingly, an object of the present invention is to reduce the breathing rate and improve the permeability in the case of using a calcium-containing substance such as granulated blast furnace slag as a grout injector by directly utilizing the excellent hydraulic property. It is in.

【0009】[0009]

【課題を解決するための手段】上記課題を解決した本発
明のグラウト注入剤は、酸化カルシウムの含有量が20
〜50重量%であり、内部構造の90%以上がガラス質
であり、かつブレーン値が5000cm2 /g以上の微粉末に対
して、海水または海水混入地下水を添加した懸濁液であ
ことを特徴とするものである
In order to achieve the object of the present onset which the above-mentioned problems are eliminated
Ming grout filler has a calcium oxide content of 20
A 50% by weight, suspension der more than 90% of the internal structure is glassy, and Blaine value relative to the fine powder of more than 5000 cm 2 / g, was added seawater or seawater contamination groundwater
It is characterized in that that.

【0010】[0010]

【作用】本発明に従って、高炉水砕スラグなどの酸化カ
ルシウム含有物に対して、海水または海岸近傍に地下水
を添加すると、海水または海岸近傍の地下水に含有する
各イオンの電位により、高炉水砕スラグ微粒子が反発す
るようになり、粒子の沈降性を抑制するために、ブリー
ジング率が小さくなる。また、高炉水砕スラグ微粒子の
加水分解を促進させ、強度の高い固結体を得ることがで
きる。
According to the present invention, when groundwater is added to seawater or near the coast to calcium oxide-containing substances such as granulated blast furnace slag, the potential of each ion contained in the seawater or groundwater near the coast increases the blast furnace granulated slag. The fine particles come to repel, and the breathing rate decreases in order to suppress the sedimentation of the particles. Further, the hydrolysis of the granulated blast furnace slag particles is promoted, and a solidified body having high strength can be obtained.

【0011】[0011]

【実施例】以下本発明を具体的にさらに詳説する。本発
明では、酸化カルシウムの含有量が20〜50重量%で
あり、内部構造の90%以上がガラス質であり、ブレー
ン値が5000cm2 /g以上の微粉末を用いる。
Now, the present invention will be described in further detail with reference to Examples. In the present invention, a fine powder having a calcium oxide content of 20 to 50% by weight, 90% or more of the internal structure being vitreous, and having a Blaine value of 5000 cm 2 / g or more is used.

【0012】この代表例としては、高炉水砕スラグの微
粉末を挙げることができる。他の冶金スラグも用いるこ
とができる。酸化カルシウムの含有量はより好ましくは
25〜35重量%である。ブレーン値としては、浸透性
の点でより好ましくは8000〜16000cm2 /g である。粗大
な粒子の場合、地盤中に対する浸透性が悪い。ブレーン
値がより高くとも、浸透性の向上はさほど期待できず、
また粉砕に要するコストの増大を招く。
As a typical example, fine powder of granulated blast furnace slag can be mentioned. Other metallurgical slags can also be used. The content of calcium oxide is more preferably 25 to 35% by weight. The Blaine value is more preferably 8000 to 16000 cm 2 / g in terms of permeability. In the case of coarse particles, permeability to the ground is poor. Even with a higher Blaine value, there is not much improvement in permeability,
In addition, the cost required for pulverization is increased.

【0013】この種の高炉水砕スラグに対して、海水ま
たは海岸近傍の地下水が添加される。高炉水砕スラグ微
粒子を清水に懸濁させて、これに海水または海岸近傍の
地下水添加してもよいが、直接海水または海岸近傍の
地下水に高炉水砕スラグ微粒子を懸濁させることもでき
る。高炉水砕スラグは懸濁液中に100〜700kg/m
3 分散しているのが好ましい。
[0013] Seawater or groundwater near the coast is added to this type of granulated blast furnace slag. Was suspended granulated blast furnace slag fine Shimizu, this may be added the groundwater seawater or coast near, but may also be suspended the granulated blast furnace slag fine groundwater directly seawater or shore near. Granulated blast furnace slag is 100-700kg / m in suspension
Preferably 3 are dispersed.

【0014】いずれにしても、懸濁液中に次記のよう
に、1リットル中に各イオンが存在することが好まし
い。 <中性領域の硬化反応促進液> Na+ : 10000〜100000 mg 、 Cl- :10000 〜 50000 mg K+ : 200〜 10000 mg 、 SO4 - : 3000 〜 10000 mg Ca2+: 200〜 20000 mg 、SiO3 - : 5000 〜100000 mg Mg2+: 200〜 50000 mg 、HCO3 - : 2000 〜 20000 mg Al3+: 200〜 50000 mg <弱アルカリ領域の硬化反応促進液> Na+ :100000〜1000000 mg 、 Cl- : 10000〜 50000 mg K+ : 200〜 10000 mg 、 SO4 - : 5000〜 50000 mg Ca2+: 20000〜 100000 mg 、SiO3 - :100000〜500000 mg Mg2+: 50000〜 150000 mg 、HCO3 - : 20000〜200000 mg Al3+: 200〜 50000 mg 本発明係るグラウト注入剤は、通常、各材料を予め調
合し一液で対象地盤注入する。
In any case, it is preferable that each ion is present in one liter of the suspension as described below. <Curing reaction accelerating liquid neutral region> Na +: 10000~100000 mg, Cl -: 10000 ~ 50000 mg K +: 200~ 10000 mg, SO 4 -: 3000 ~ 10000 mg Ca 2+: 200~ 20000 mg, SiO 3 -: 5000 ~100000 mg Mg 2+: 200~ 50000 mg, HCO 3 -: 2000 ~ 20000 mg Al 3+: < curing reaction accelerating liquid of weak alkali region> 200~ 50000 mg Na +: 100000~1000000 mg , Cl -: 10000~ 50000 mg K +: 200~ 10000 mg, SO 4 -: 5000~ 50000 mg Ca 2+: 20000~ 100000 mg, SiO 3 -: 100000~500000 mg mg 2+: 50000~ 150000 mg, HCO 3 -: 20000~200000 mg Al 3+ : grouting agent according to 200 to 50000 mg present invention is usually injected into the target ground in advance formulated one-pack the materials.

【0015】〔実施例〕 以下に実施例を示し本発明の効果を明らかにする。高炉
水砕スラグの微粉末(ブレーン値15000cm2 /g)を、水道
水(清水)、中性領域の海水、弱アルカリ性領域の海水
を添加し、高炉水砕スラグが200kg/m3 の懸濁液を
豊浦標準砂を充填したモルードに注入し、ブリージング
率、凝結時間、浸透性(50cm浸透するのに要する時
間)、サンドゲルの3日強度、材令に対する強度変化を
調べたところ、図1〜図5に示す結果を得た。本発明に
したがって、海水または海岸近傍の地下水を添加する
と、浸透性が改善され、強度が向上し、強度はポルトラ
ンドセメントと同様となることが判明した。
[Examples] Examples will be shown below to clarify the effects of the present invention. Fine powder of granulated blast furnace slag (the Blaine value 15000 cm 2 / g), tap water (Shimizu), seawater neutral region, was added to seawater weakly alkaline region, suspension granulated blast furnace slag is 200 kg / m 3 When injecting the liquid into Toyoura Morudo filled with standard sand, breathing rate, setting time, (time required to be 50cm penetration) permeability were examined 3 days strength of Sandogeru, the intensity change to wood age, 1 to The result shown in FIG. 5 was obtained. It has been found that the addition of seawater or groundwater near the coast according to the present invention improves permeability, increases strength, and is similar in strength to Portland cement.

【0016】[0016]

【発明の効果】以上の通り、本発明によれば、高炉水砕
スラグなどのカルシウム含有物の優れた水硬性をそのま
ま利用してグラウト注入剤とする場合において、ブリー
ジング率を低下させ、浸透性の改良を図ることができ
る。
As described above, according to the present invention, when a grout injecting agent is used by directly utilizing the excellent hydraulic property of a calcium-containing material such as granulated blast furnace slag, the bleeding rate is reduced and the permeability is reduced. Can be improved.

【図面の簡単な説明】[Brief description of the drawings]

【図1】懸濁液の相違によるブリージング率を示す棒グ
ラフである。
FIG. 1 is a bar graph showing the breathing rate according to the difference in suspension.

【図2】懸濁液の相違による凝結時間を示す棒グラフで
ある。
FIG. 2 is a bar graph showing the setting time for different suspensions.

【図3】懸濁液の相違による浸透性を示す棒グラフであ
る。
FIG. 3 is a bar graph showing the permeability of different suspensions.

【図4】懸濁液の相違によるサンドゲルの3日強度を示
す棒グラフである。
FIG. 4 is a bar graph showing the 3-day strength of a sandgel with different suspensions.

【図5】懸濁液の相違による材令に対する強度変化のグ
ラフである。
FIG. 5 is a graph showing the change in strength with age due to the difference in suspension.

フロントページの続き (58)調査した分野(Int.Cl.6,DB名) C09K 17/02 C04B 28/08 E02D 3/12 101Continuation of the front page (58) Field surveyed (Int.Cl. 6 , DB name) C09K 17/02 C04B 28/08 E02D 3/12 101

Claims (1)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】酸化カルシウムの含有量が20〜50重量
%であり、内部構造の90%以上がガラス質であり、
ブレーン値が5000cm2 /g以上の微粉末に対して、海水
または海水混入地下水を添加した懸濁液であることを特
徴とするグラウト注入剤
1. The method according to claim 1, wherein the content of calcium oxide is 20 to 50% by weight, and 90% or more of the internal structure is glassy .
A grout filler comprising a suspension obtained by adding seawater or groundwater mixed with seawater to a fine powder having a brane value of 5000 cm 2 / g or more.
JP6049291A 1991-03-25 1991-03-25 Grout injection Expired - Fee Related JP2860716B2 (en)