JP2006024754A - Wiring layer, forming method thereof, and thin-film transistor - Google Patents

Wiring layer, forming method thereof, and thin-film transistor Download PDF

Info

Publication number
JP2006024754A
JP2006024754A JP2004201683A JP2004201683A JP2006024754A JP 2006024754 A JP2006024754 A JP 2006024754A JP 2004201683 A JP2004201683 A JP 2004201683A JP 2004201683 A JP2004201683 A JP 2004201683A JP 2006024754 A JP2006024754 A JP 2006024754A
Authority
JP
Japan
Prior art keywords
layer
copper
wiring layer
metal
seed layer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2004201683A
Other languages
Japanese (ja)
Inventor
Hiroyoshi Nakamura
弘喜 中村
Masateru Kado
昌輝 門
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Advanced LCD Technologies Development Center Co Ltd
Original Assignee
Advanced LCD Technologies Development Center Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Advanced LCD Technologies Development Center Co Ltd filed Critical Advanced LCD Technologies Development Center Co Ltd
Priority to JP2004201683A priority Critical patent/JP2006024754A/en
Publication of JP2006024754A publication Critical patent/JP2006024754A/en
Pending legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To obtain a specific resistance of 2.5 μΩcm or smaller, even for a thin film in which the wiring film thickness is in sub μm order of approximately 200-1,000 nm, and to provide a method for forming a wiring layer and to provide the wiring layer. <P>SOLUTION: In the wiring layer, a silicon nitride film in a substrate insulating film 2 is formed on a glass substrate 1, a substrate metal layer 3 is formed on it, a metal seed layer 4 is formed on it, and a metal wiring layer 7 is formed on the metal seed layer 4. In the wiring layer, the crystal surface of the metal seed layer 4 is orientated mainly in the (111) orientation, the average crystal particle diameter is 0.25 μm or larger, and the film thickness of the metal wiring layer is 200-1,000 nm and is formed by an electroless plating method. <P>COPYRIGHT: (C)2006,JPO&NCIPI

Description

本発明は、低抵抗に形成される配線層の形成方法、配線層および薄膜トランジスタに関するものである。   The present invention relates to a method for forming a wiring layer formed with low resistance, a wiring layer, and a thin film transistor.

一般に、LSIやULSIに代表される半導体装置における配線や電極の材料としては、主としてアルミニウム(Al)やその合金などが用いられている。しかし、近年の集積度の向上による微細化の進展や、動作スピードの向上等により、Alよりも抵抗が低く、且つエレクトロマイグレーションやストレスマイグレーション等の耐性が高い特性を有する銅(Cu)を次世代の配線及び電極の材料として採用することを目的として開発が進められている。   Generally, aluminum (Al) or an alloy thereof is mainly used as a material for wiring and electrodes in a semiconductor device represented by LSI or ULSI. However, due to the progress of miniaturization due to the recent improvement in integration and the improvement of the operation speed, the next generation of copper (Cu), which has lower resistance than Al and higher resistance to electromigration and stress migration, etc. Development is underway for the purpose of adopting it as a material for wiring and electrodes.

さらに、例えば液晶表示装置等に代表される表示装置の分野においても、表示面積の拡大による配線長の増加や、駆動用ドライバ回路や画素内メモリといった様々な付加機能を搭載するモノリシック化等の要求や、デジタル時代に適合した大容量・大画面・高精細の液晶表示装置等によって、半導体分野と同様に低抵抗な配線が要求されている。   Furthermore, in the field of display devices such as liquid crystal display devices, for example, there is a demand for increasing the wiring length by expanding the display area, and monolithic mounting with various additional functions such as a driver circuit for driving and an in-pixel memory. In addition, low-resistance wiring is required in the same manner as in the semiconductor field due to large capacity, large screen, and high-definition liquid crystal display devices suitable for the digital age.

銅の微細な配線加工は、Al配線の形成技術と同様に、PEP(Photo Engraving Process:写真食刻工程、所謂フォトリソグラフィー)によるマスキング技術と、RIE(Reactive Ion Etching:反応性イオンエッチング)法等のエッチング技術とを単に組み合わせても、実現が困難であった。つまり、銅のハロゲン化物の蒸気圧は、Alに対して非常に低く(即ち、蒸発しにくい)、RIE等のエッチング技術を用いる場合には、プロセス温度として200〜300℃に温調された雰囲気下でのエッチング処理が必要である等、種々の課題が多い。また、通常のフォトレジストマスクではなく、SiOやSiNxによるマスクを使用する必要もある。銅の微細な配線加工は、例えば、ダマシン法と呼ばれている方法で、特許文献1や特許文献2に開示されている。 Copper fine wiring processing, like Al wiring formation technology, masking technology using PEP (Photo Engraving Process, so-called photolithography), RIE (Reactive Ion Etching) method, etc. Even if this etching technique is simply combined, it has been difficult to realize. In other words, the vapor pressure of copper halide is very low (ie, difficult to evaporate) with respect to Al, and when an etching technique such as RIE is used, the process temperature is adjusted to 200 to 300 ° C. There are many problems such as the necessity of an etching process below. Further, it is necessary to use a mask made of SiO 2 or SiNx instead of a normal photoresist mask. The fine wiring processing of copper is disclosed in Patent Document 1 and Patent Document 2 by a method called a damascene method, for example.

このダマシン法による銅の微細な配線加工は、次のような工程を経て加工されている。即ち、まず、基板上の絶縁層に対して、あらかじめ所望の配線パターンの配線溝を形成する。次に、銅の酸化シリコン層中への拡散を防止するために銅薄層の下地層としてTaN、Ta、TiN、等の銅拡散防止層を形成する。この銅拡散防止層上に銅薄層を形成する方法である。この銅薄層は、配線溝を埋め込むようにスパッタリング法等のPVD(PHYSICAL VAPOR DEPOSITION)法、めっき法又は、有機金属材料を用いたCVD(CHEMICAL VAPOR DEPOSITION:化学気相成長)法等の種々の手法を用いて、溝内部に埋め込み且つ絶縁層上の全面に亘って形成する。その後、銅薄層を基板表面側から下層の絶縁層が露出する(溝部分の開口端面)までCMP(CHEMICAL MECHANICAL POLISING:化学的機械研磨法)等の研磨法やエッチバック等を用いて除去し、溝に埋め込まれた銅のみによる配線パターンを形成する。更に、銅配線上に銅拡散防止能を有する絶縁層もしくは金属層を形成して銅配線層を覆う方法である。
特開2001−189295公報 特開平11−135504号公報
The fine wiring process of copper by this damascene method is processed through the following steps. That is, first, a wiring groove having a desired wiring pattern is formed in advance on the insulating layer on the substrate. Next, in order to prevent the diffusion of copper into the silicon oxide layer, a copper diffusion prevention layer such as TaN, Ta, TiN or the like is formed as a base layer of the thin copper layer. In this method, a thin copper layer is formed on the copper diffusion prevention layer. This copper thin layer is formed by various methods such as PVD (PHYSICAL VAPOR DEPOSITION) method such as sputtering method, plating method or CVD (CHEMICAL VAPOR DEPOSITION) method using an organic metal material so as to fill the wiring groove. Using a technique, it is embedded in the groove and formed over the entire surface of the insulating layer. After that, the thin copper layer is removed using a polishing method such as CMP (CHEMICAL MECHANICAL POLISING) or etch back until the underlying insulating layer is exposed from the substrate surface side (open end face of the groove). Then, a wiring pattern made only of copper embedded in the groove is formed. Furthermore, it is a method of covering the copper wiring layer by forming an insulating layer or a metal layer having a copper diffusion preventing ability on the copper wiring.
JP 2001-189295 A Japanese Patent Laid-Open No. 11-135504

しかしながら、前述した公報に開示された技術を含む従来技術には以下に挙げるような課題がある。上記ダマシン法においては、少なくとも配線を埋め込むための溝を形成する溝加工工程、金属拡散防止層、金属シード層、金属配線層及び研磨停止膜を形成するための成膜工程、フォトリソグラフィー工程、エッチング工程、研磨工程などが必要であり、製造工程が煩雑となり、製造コストが高くなる。 However, the conventional techniques including the technique disclosed in the above publication have the following problems. In the damascene method, at least a groove processing step for forming a groove for embedding wiring, a metal diffusion prevention layer, a metal seed layer, a metal wiring layer, and a film formation step for forming a polishing stopper film, a photolithography step, etching A process, a grinding | polishing process, etc. are required, a manufacturing process becomes complicated and manufacturing cost becomes high.

また、配線抵抗を低減するためには、配線の断面積を大きくする必要があるが、集積化の制約から、アスペクト比の高い(つまり、幅や径が狭く深い)溝やビアホールを採用すると、銅の埋め込み性が低下する。配線抵抗を低減するためにLSIでは、膜厚をμmオーダの厚い膜を形成している。しかし、薄膜トランジスタ(TFT)回路では、サブμmオーダの膜厚が要求され、このオーダの膜厚では比抵抗が2.5μΩcm以下の銅配線を得ることが難しい。また、銅薄層を基板全面に成膜した後に、不要部分を除去するというCMP工程等は、処理時間が掛かり、スループットが悪い課題がある。   In order to reduce the wiring resistance, it is necessary to increase the cross-sectional area of the wiring. However, due to the limitation of integration, if a groove or via hole with a high aspect ratio (that is, a narrow width and diameter) is used, Copper embedding is reduced. In order to reduce the wiring resistance, in LSI, a film having a thickness of the order of μm is formed. However, a thin film transistor (TFT) circuit requires a thickness of the order of sub-μm, and it is difficult to obtain a copper wiring having a specific resistance of 2.5 μΩcm or less with this order of thickness. In addition, a CMP process or the like of removing unnecessary portions after forming a thin copper layer on the entire surface of the substrate requires processing time and has a problem of poor throughput.

さらに、直径12インチ等の大口径半導体ウエハサイズに対応する大型のCMP装置が開発されているが、上記半導体ウエハよりも大面積で且つ平坦性等の精度の悪いガラス基板を用いる表示装置のための製造装置は実用化されていない。また、長辺が1m以上の大型ガラス基板を用いた表示装置の製造の場合、上記CMPによる全面研磨やエッチング法による除去が可能であったとしても、配線として利用される銅薄層部分の面積は、ガラス基板の面積に比較して非常に小さいために、成膜された銅薄層の大部分は除去され、廃棄される。この結果、高価な銅の利用効率は非常に悪くなり、高コストになる影響で製品価格も高くなる。   Furthermore, although a large-sized CMP apparatus corresponding to a large-diameter semiconductor wafer size such as 12 inches in diameter has been developed, for a display apparatus using a glass substrate having a larger area and lower flatness than the semiconductor wafer. This manufacturing apparatus has not been put into practical use. Further, in the case of manufacturing a display device using a large glass substrate having a long side of 1 m or more, the area of the copper thin layer portion used as the wiring even if the entire surface polishing by CMP or the etching method can be removed. Is very small compared to the area of the glass substrate, so that most of the deposited copper thin layer is removed and discarded. As a result, the utilization efficiency of expensive copper becomes very poor, and the product price increases due to the high cost.

配線材料の銅の利用効率を向上するために、本発明者らはレジストを用いた選択無電解銅めっきプロセスの開発を行っている。この無電解銅めっき配線形成プロセスは、無電解銅めっき膜の形成前にスパッタリング法により銅シード層(以下スパッタ銅シード層と略す。)を形成し、この上に配線パターンのレジスト溝を形成し、その溝に無電解めっきにより銅配線層を形成し、その後、配線パターンのレジスト膜を除去した後、銅シード層をエッチングする方法である。この無電解銅めっき膜形成プロセスは、液晶等の表示装置で用いられる300〜600nm程度の低配線厚でも低比抵抗値の銅配線薄膜を形成できる。しかし、300〜600nm程度の低配線厚の配線を無電解めっき法で形成する場合、銅配線層の比抵抗値は銅シード層の結晶性に大きく依存するという問題がある。銅配線は、比抵抗値が高ければ、銅配線を用いる意味がないため、膜厚が200〜1000nm程度のサブμmオーダの配線でも2.5μΩcm以下の比抵抗値を実現することが必要条件である。   In order to improve the utilization efficiency of copper as a wiring material, the present inventors have developed a selective electroless copper plating process using a resist. In this electroless copper plating wiring formation process, a copper seed layer (hereinafter abbreviated as a sputtered copper seed layer) is formed by sputtering before forming an electroless copper plating film, and a resist groove of a wiring pattern is formed thereon. In this method, a copper wiring layer is formed in the groove by electroless plating, the resist film of the wiring pattern is removed, and then the copper seed layer is etched. This electroless copper plating film forming process can form a copper wiring thin film having a low specific resistance value even with a low wiring thickness of about 300 to 600 nm used in a display device such as a liquid crystal. However, when a wiring having a low wiring thickness of about 300 to 600 nm is formed by an electroless plating method, there is a problem that the specific resistance value of the copper wiring layer largely depends on the crystallinity of the copper seed layer. If the copper wiring has a high specific resistance value, it is meaningless to use the copper wiring. Therefore, it is necessary to realize a specific resistance value of 2.5 μΩcm or less even in a sub-μm order wiring having a film thickness of about 200 to 1000 nm. is there.

無電解めっき法で通常用いられるPd触媒核を用いずにスパッタ銅シード層を用いる理由は、Pd触媒核から成長させる無電解めっきでは、銅はPd核の周囲に成長してPd核を中心としたCu核がぶつかり合うことで配線が形成されるために配線膜厚の薄いものへの適用が難しく、Pd核密度を高める必要がある。しかしながら、Pd核密度及び均一性を制御することが難しく、更にPdが後工程の熱処理で銅中に拡散して比抵抗を高くするという問題などもありPd触媒核を用いることは問題がある。このため、当然ながら、Pd触媒を用いた無電解めっき法で銅シード層を形成する方法も同様な問題を有していて、加えてバリア性を有する下地金属層との密着性が低いという問題も有している。 The reason why the sputtered copper seed layer is used without using the Pd catalyst nucleus normally used in the electroless plating method is that, in the electroless plating grown from the Pd catalyst nucleus, the copper grows around the Pd nucleus and centers on the Pd nucleus. Since the Cu nuclei collide with each other to form a wiring, it is difficult to apply to a thin wiring film, and it is necessary to increase the Pd nucleus density. However, it is difficult to control the density and uniformity of Pd nuclei, and there is a problem that Pd diffuses into copper by heat treatment in a later process to increase the specific resistance. For this reason, of course, the method of forming the copper seed layer by the electroless plating method using the Pd catalyst also has the same problem, and in addition, the problem of low adhesion to the underlying metal layer having barrier properties. Also have.

本発明は、上記問題点に対処してなされたもので、配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる配線層の形成方法、配線層および薄膜トランジスタを提供することを目的とする。   The present invention has been made in response to the above problems, and a wiring layer forming method and wiring capable of obtaining a specific resistance of 2.5 μΩcm or less even with a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm. It is an object to provide a layer and a thin film transistor.

上記課題を解決するために、本発明の配線層の形成方法、配線層および薄膜トランジスタは、主結晶面が(111)で、平均結晶粒径が0.25μm以上の金属シード層を設け、この金属シード層上に、膜厚が200乃至1000nmの金属配線層を無電解めっきして設けられた膜を有するものである。   In order to solve the above problems, the wiring layer forming method, wiring layer and thin film transistor of the present invention are provided with a metal seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more. On the seed layer, there is a film provided by electroless plating a metal wiring layer having a thickness of 200 to 1000 nm.

本発明の配線層の形成方法は、主結晶面が(111)で、平均結晶粒径が0.25μm以上の金属シード層を形成する工程と、前記金属シード層上に膜厚が200乃至1000nmの金属配線層を無電解めっきする工程とを具備してなることを特徴とする。この配線層の形成方法によれば配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる。   The wiring layer forming method of the present invention includes a step of forming a metal seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more, and a film thickness of 200 to 1000 nm on the metal seed layer. And a step of electrolessly plating the metal wiring layer. According to this method for forming a wiring layer, a specific resistance of 2.5 μΩcm or less can be obtained even in a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm.

本発明の配線層の形成方法は、主結晶面が(111)で、平均結晶粒径が0.25μm以上の銅シード層を形成する工程と、前記銅シード層上に膜厚が200乃至1000nmの銅配線層を無電解めっきする工程とを具備してなることを特徴とする。この配線層の形成方法によれば銅配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる。   The wiring layer forming method of the present invention includes a step of forming a copper seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more, and a film thickness of 200 to 1000 nm on the copper seed layer. And a step of electrolessly plating the copper wiring layer. According to this method for forming a wiring layer, a specific resistance of 2.5 μΩcm or less can be obtained even in a sub-μm order thin film having a copper wiring film thickness of about 200 to 1000 nm.

本発明の配線層の形成方法は、基板上に下地金属層を形成する工程と、前記下地金属層上に主結晶面が(111)で、平均結晶粒径が0.25μm以上の銅シード層を形成する工程と、前記銅シード層上に膜厚が200乃至1000nmで予め定められたパターンの銅配線層を無電解めっきする工程と、少なくとも前記銅配線層と接合される領域以外の前記銅シード層および前記下地金属層を除去する工程とを具備してなることを特徴とする。この配線層の形成方法によれば銅配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる。さらに、下地金属層の金属を選択することにより銅配線層の平均結晶粒径を大きくすることができる。   The wiring layer forming method of the present invention includes a step of forming a base metal layer on a substrate, and a copper seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more on the base metal layer. Forming a copper wiring layer having a predetermined thickness of 200 to 1000 nm on the copper seed layer, and at least the copper other than the region bonded to the copper wiring layer And a step of removing the seed layer and the base metal layer. According to this method for forming a wiring layer, a specific resistance of 2.5 μΩcm or less can be obtained even in a sub-μm order thin film having a copper wiring film thickness of about 200 to 1000 nm. Furthermore, the average crystal grain size of the copper wiring layer can be increased by selecting the metal of the base metal layer.

本発明の配線層は、金属シード層上に金属配線層が設けられた配線層であって、前記金属シード層は主結晶面が(111)で、平均結晶粒径が0.25μm以上であり、前記金属配線層は膜厚が200乃至1000nmであり、無電解めっきされた層であることを特徴とする。この配線層によれば配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる。さらに、1m以上の大きな基板でも低比抵抗の銅配線層を形成することができる。   The wiring layer of the present invention is a wiring layer in which a metal wiring layer is provided on a metal seed layer, and the metal seed layer has a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more. The metal wiring layer has a thickness of 200 to 1000 nm and is an electroless plated layer. According to this wiring layer, a specific resistance of 2.5 μΩcm or less can be obtained even in a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm. Furthermore, a copper wiring layer having a low specific resistance can be formed even on a large substrate of 1 m or more.

本発明の薄膜トランジスタは、結晶化領域を有する半導体薄膜と、前記結晶化領域内にソース領域およびドレイン領域が設けられ、前記結晶化領域にゲート絶縁膜を介して設けられたゲート電極を有する薄膜トランジスタとを具備し、前記薄膜トランジスタのソース電極、ドレイン電極、ゲート電極の少なくとも1つの電極は主結晶面が(111)で、平均結晶粒径が0.25μm以上の金属シード層と、この金属シード層上に設けられた膜厚が200乃至1000nmの無電解めっき層とで構成したものであることを特徴とする。この薄膜トランジスタによれば配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗の電極や配線の少なくとも一方を得ることができる。さらに、1m以上の大きな基板でも低比抵抗の電極や配線層の少なくとも一方を形成することができる。   The thin film transistor of the present invention includes a semiconductor thin film having a crystallization region, a thin film transistor having a gate electrode provided in the crystallization region with a source region and a drain region, and a gate insulating film provided in the crystallization region. And at least one of the source electrode, drain electrode, and gate electrode of the thin film transistor has a metal seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more, and on the metal seed layer The electroless plating layer having a thickness of 200 to 1000 nm is provided on the substrate. According to this thin film transistor, it is possible to obtain at least one of an electrode and a wiring having a specific resistance of 2.5 μΩcm or less even if the wiring film thickness is a sub-μm order thin film of about 200 to 1000 nm. Furthermore, at least one of a low specific resistance electrode and a wiring layer can be formed even on a large substrate of 1 m or more.

金属シード層は主結晶面が(111)とは、X線回折により検出される(111)ピークが(200)ピークよりも大きいことを意味し、望ましくはその強度比I(111)/I(200)が10以上であることが望ましい。   In the metal seed layer, the main crystal plane (111) means that the (111) peak detected by X-ray diffraction is larger than the (200) peak, and preferably its intensity ratio I (111) / I ( 200) is preferably 10 or more.

本発明の方法によれば、配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得ることができる。   According to the method of the present invention, a specific resistance of 2.5 μΩcm or less can be obtained even in a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm.

次に、本発明の配線層の形成方法および配線層の実施形態を図を参照して説明する。この実施形態は、結晶面が主として(111)に配向し、平均結晶粒径が0.25μm以上の銅を主成分とする金属シード層を設け、この金属シード層上に、膜厚が200乃至1000nmのサブμmオーダの金属配線層を無電解めっきして設けた例である。銅を主成分とする金属配線例えば、薄膜トランジスタ回路での銅を主成分とする金属配線層の膜厚は、200乃至1000nmの極薄である。このような極薄な銅を主成分とする金属配線でも2.5μΩcm以下の低抵抗な配線を可能にする。   Next, a method for forming a wiring layer and an embodiment of the wiring layer according to the present invention will be described with reference to the drawings. In this embodiment, a metal seed layer mainly composed of copper having a crystal plane mainly oriented to (111) and an average crystal grain size of 0.25 μm or more is provided, and a film thickness of 200 to 200 is formed on the metal seed layer. This is an example in which a metal wiring layer having a sub-μm order of 1000 nm is provided by electroless plating. Metal wiring mainly composed of copper For example, a metal wiring layer mainly composed of copper in a thin film transistor circuit has an extremely thin film thickness of 200 to 1000 nm. Even such a metal wiring mainly composed of ultra-thin copper enables a wiring having a low resistance of 2.5 μΩcm or less.

このメカニズムは、次のように説明することができる。即ち、通常の電解銅めっきや無電解銅めっき層形成では、配線厚が1〜30μm程度と厚いためにめっき膜厚が増大すると共に結晶粒径は増大する。他方、液晶表示装置のような配線は、サブμmオーダの薄膜が要求されるために配線膜厚を厚くすることが出来ない。銅めっき配線層の比抵抗低減のためには、銅めっき配線層の結晶粒径を大きくすることにより可能となる。液晶表示装置のように銅めっき配線層の膜厚が薄い配線の形成は、特に金属シード層の結晶性が大きく影響することを見出した。即ち、サブμmオーダの薄膜で2.5μΩcm以下の低比抵抗を得るためには、金属シード層の結晶粒径を平均結晶粒径が0.25μm以上にすることにより銅めっき配線層の結晶粒径を大きくできることを見出した。銅めっき配線層の結晶粒径を大きくできることは、低抵抗の銅めっき配線層を得ることを可能にする。主として(111)に配向とは、X線回折により検出される(111)ピークが(200)ピークよりも大きいことを意味し、望ましくはその強度比I(111)/I(200)が10以上であることが望ましい。   This mechanism can be explained as follows. That is, in normal electrolytic copper plating or electroless copper plating layer formation, since the wiring thickness is as thick as about 1 to 30 μm, the plating film thickness increases and the crystal grain size increases. On the other hand, wiring such as a liquid crystal display device requires a thin film on the order of sub-μm, so that the wiring film thickness cannot be increased. Reduction of the specific resistance of the copper-plated wiring layer can be achieved by increasing the crystal grain size of the copper-plated wiring layer. It has been found that the formation of wiring with a thin copper-plated wiring layer, such as a liquid crystal display device, is greatly affected by the crystallinity of the metal seed layer. That is, in order to obtain a low specific resistance of 2.5 μΩcm or less with a thin film on the order of sub μm, the crystal grain size of the copper plating wiring layer is set by setting the crystal grain size of the metal seed layer to 0.25 μm or more. It has been found that the diameter can be increased. The ability to increase the crystal grain size of the copper-plated wiring layer makes it possible to obtain a low-resistance copper-plated wiring layer. The orientation mainly at (111) means that the (111) peak detected by X-ray diffraction is larger than the (200) peak, and preferably the intensity ratio I (111) / I (200) is 10 or more. It is desirable that

次に、配線層の形成方法を銅(Cu)配線層の形成方法に適用した実施形態を、図1および図2を参照して工程順に説明する。図1は、Cu配線層をパターンニングされた領域に成膜する準備工程を工程順に説明するための断面図である。図2は、パターンニングされた領域にCu配線層を形成する方法を工程順に説明するための断面図である。   Next, an embodiment in which the wiring layer forming method is applied to a copper (Cu) wiring layer forming method will be described in the order of steps with reference to FIGS. FIG. 1 is a cross-sectional view for explaining a preparation step for forming a Cu wiring layer in a patterned region in the order of steps. FIG. 2 is a cross-sectional view for explaining a method of forming a Cu wiring layer in a patterned region in the order of steps.

基板例えばガラス基板1上に、図1(a)に示すように下地絶縁層2例えば窒化シリコン(SiN)膜を膜厚例えば300nm形成する。このSiN膜上に、図1(b)に示すように銅のバリア膜としても有効な下地金属層3例えばタンタル(Ta)層を例えばスパッタ法により形成する。膜厚は、例えばTa層を50nmに形成するとよい。下地金属層3としては、Ta層のほかβ−Ta,α−Ta,TaSiN,TaN,TaNとα−Taの積層膜のうち少なくも一つの材料層により構成されていることが望ましい。さらに、この下地金属層3上に、図1(c)に示すように金属シード層4例えば銅を主成分とする金属シード層を形成する。銅を主成分とする金属シード層は、厚さ例えば50nmを例えばスパッタ法により形成する。この銅を主成分とする金属シード層は、結晶方位が主として(111)に配向し、平均結晶粒径が0.25μm以上である。   A base insulating layer 2 such as a silicon nitride (SiN) film is formed on a substrate such as a glass substrate 1 as shown in FIG. On this SiN film, as shown in FIG. 1B, a base metal layer 3 such as a tantalum (Ta) layer that is also effective as a copper barrier film is formed by, for example, sputtering. Regarding the film thickness, for example, a Ta layer is preferably formed to 50 nm. The base metal layer 3 is preferably composed of at least one material layer among the laminated films of β-Ta, α-Ta, TaSiN, TaN, TaN and α-Ta in addition to the Ta layer. Further, a metal seed layer 4, for example, a metal seed layer mainly composed of copper is formed on the base metal layer 3 as shown in FIG. The metal seed layer mainly composed of copper is formed with a thickness of, for example, 50 nm, for example, by sputtering. The metal seed layer containing copper as a main component has a crystal orientation mainly oriented in (111) and an average crystal grain size of 0.25 μm or more.

銅のバリア膜としても有効な下地金属層3としてTa層は、この積層膜上に平均結晶粒径の大きな金属シード層4を形成するのに有効である。平均結晶粒径が0.25μm以上の上記金属シード層4は、この金属シード層4上に低比抵抗の金属配線層7の成膜を可能にする。   The Ta layer as the base metal layer 3 that is also effective as a copper barrier film is effective in forming the metal seed layer 4 having a large average crystal grain size on the laminated film. The metal seed layer 4 having an average crystal grain size of 0.25 μm or more enables a metal wiring layer 7 having a low specific resistance to be formed on the metal seed layer 4.

上記金属シード層4上に、図1(d)に示すように配線のための材料を予め定められた配線パターン領域のみに形成するためにフォトレジスト層5を成膜する。このフォトレジスト層5の成膜は、例えばスピンコート法により膜厚例えば1.2μm形成する。フォトレジスト層5の膜厚は、金属配線層7の膜厚以上の厚さを選択する。このようにして配線層を配線パターン領域のみに形成するための準備工程を終了する。 A photoresist layer 5 is formed on the metal seed layer 4 in order to form a wiring material only in a predetermined wiring pattern region as shown in FIG. The photoresist layer 5 is formed, for example, by a spin coating method to a film thickness of 1.2 μm, for example. The thickness of the photoresist layer 5 is selected to be greater than or equal to the thickness of the metal wiring layer 7. In this way, the preparation process for forming the wiring layer only in the wiring pattern region is completed.

次に、図2を参照して、パターンニングされた領域に銅を主成分とする金属配線層を形成する方法を工程順に説明する。予め定められた電極パターンや所望の配線形成パターンのマスク像を上記フォトレジスト層5に投影し露光する。露光後、次に、現像工程を実施することにより図2(a)に示すようにフォトレジスト層5には、配線パターン領域の溝パターン6が形成される。この状態で溝パターン6の底面には、金属シード層4の表面が露出する。   Next, a method for forming a metal wiring layer mainly composed of copper in a patterned region will be described in the order of steps with reference to FIG. A mask image of a predetermined electrode pattern or a desired wiring formation pattern is projected onto the photoresist layer 5 and exposed. After the exposure, a development process is then performed to form a groove pattern 6 in the wiring pattern region in the photoresist layer 5 as shown in FIG. In this state, the surface of the metal seed layer 4 is exposed on the bottom surface of the groove pattern 6.

次に、この溝パターン6に金属配線層7を図2(b)に示すように成膜する。この成膜法は、例えば無電解めっき法により銅を主成分とする金属配線層7を厚さ200〜1000nmの極めて薄い膜厚例えば300nm形成する。即ち、主として結晶方位(111)に配向した銅シード層上に銅めっき層がエピタキシャル成長する。このとき銅シード層の平均結晶粒径と銅めっき層の平均結晶粒径は、ほぼ等しい。平均結晶粒径の大きな銅シード層上の方が、めっき条件に係わらず銅めっき層の結晶粒径は大きくなる。もちろん、無電解めっき法による金属配線層7の形成の前処理として、金属シード層4の表面の酸化物を除去する洗浄工程を付加することが望ましい。   Next, a metal wiring layer 7 is formed in the groove pattern 6 as shown in FIG. In this film forming method, the metal wiring layer 7 mainly composed of copper is formed by an electroless plating method, for example, by forming an extremely thin film thickness of 200 nm to 1000 nm, for example, 300 nm. That is, a copper plating layer is epitaxially grown on a copper seed layer mainly oriented in the crystal orientation (111). At this time, the average crystal grain size of the copper seed layer and the average crystal grain size of the copper plating layer are substantially equal. The crystal grain size of the copper plating layer is larger on the copper seed layer having a larger average crystal grain size regardless of the plating conditions. Of course, as a pretreatment for forming the metal wiring layer 7 by the electroless plating method, it is desirable to add a cleaning process for removing the oxide on the surface of the metal seed layer 4.

このように極めて薄い銅を主成分とする金属配線層7を形成するための無電解めっき浴としては、例えばコバルト塩を還元剤とする中性無電解めっき浴を用いることが望ましい。中性無電解めっき浴組成としては、還元剤としては例えば硫酸コバルトもしくは硝酸コバルト、銅塩として例えば硫酸銅もしくは硝酸銅、錯化剤としてエチレンジアミン、還元剤助剤として例えばアスコルビン酸、錯化剤助剤として例えば2,2’−ビピリジル、反応開始剤として例えば塩酸を用いるとよい。コバルト塩を還元剤とする中性無電解めっき浴は、pH領域が6〜7程度であるため通常のフォトレジストを用いることができることに加え、有害物質やアルカリ金属も含まないために液晶表示装置のような薄膜トランジスタの製造工程にも適用が可能であるという利点がある。 As such an electroless plating bath for forming the metal wiring layer 7 mainly composed of extremely thin copper, it is desirable to use, for example, a neutral electroless plating bath using a cobalt salt as a reducing agent. The composition of the neutral electroless plating bath is, for example, cobalt sulfate or cobalt nitrate as a reducing agent, copper sulfate or copper nitrate as a copper salt, ethylenediamine as a complexing agent, ascorbic acid or complexing agent as a reducing agent, and the like. For example, 2,2′-bipyridyl may be used as an agent, and hydrochloric acid may be used as a reaction initiator. Since the neutral electroless plating bath using a cobalt salt as a reducing agent has a pH range of about 6 to 7, in addition to being able to use a normal photoresist, it does not contain harmful substances or alkali metals. There is an advantage that it can be applied to the manufacturing process of the thin film transistor.

無電解めっきによる銅を主成分とする金属配線層7の成膜は、大きさ1m以上の液晶表示装置用ガラス基板への薄膜の成膜を可能にする。サブμmオーダの薄膜でも2.5μΩcm以下の比抵抗を得るための銅を主成分とする金属配線層7の結晶粒径は、平均結晶粒径が0.25μm以上であることが重要である。さらに、溝パターン6のみに銅めっき層を無電解めっきすることは、銅を不要な部分に成膜しないため、省資源効果のある製造方法である。 Formation of the metal wiring layer 7 containing copper as a main component by electroless plating enables formation of a thin film on a glass substrate for a liquid crystal display device having a size of 1 m or more. In order to obtain a specific resistance of 2.5 μΩcm or less even in a sub-μm order thin film, it is important that the crystal grain size of the metal wiring layer 7 containing copper as a main component is an average crystal grain size of 0.25 μm or more. Further, electroless plating of the copper plating layer only on the groove pattern 6 is a manufacturing method having a resource saving effect because copper is not formed on unnecessary portions.

次に、図2(c)に示すようにフォトレジスト層5を除去する。この結果、表面には、銅を主成分とする金属配線層7と金属シード層4とが露出する。次に、金属配線層7をマスクとして金属シード層4をエッチングして除去する。さらに、金属配線層7をマスクとして図2(d)に示すように下地金属層3をエッチングして除去する。この結果、SiN膜の表面に銅を主成分とする金属配線層7のパターンが形成された基板8を得ることができる。 Next, as shown in FIG. 2C, the photoresist layer 5 is removed. As a result, the metal wiring layer 7 and the metal seed layer 4 mainly composed of copper are exposed on the surface. Next, the metal seed layer 4 is etched and removed using the metal wiring layer 7 as a mask. Further, using the metal wiring layer 7 as a mask, the base metal layer 3 is removed by etching as shown in FIG. As a result, the substrate 8 in which the pattern of the metal wiring layer 7 mainly composed of copper is formed on the surface of the SiN film can be obtained.

上記銅を主成分とする金属配線層7は、配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の低比抵抗を得ることができる。上記のコバルト塩を還元剤する中性無電解めっき浴を用いた銅配線層の形成において、銅めっき層の結晶方位は金属シード層4の結晶方位に依存し、かつ、金属配線層7の膜厚が300nm程度と薄い場合は銅めっき層の平均結晶粒径は金属シード層4とほぼ同等であることを本発明者らは見出した。即ち、金属シード層4の結晶粒径を2.5μΩcm以下の低比抵抗を得るための結晶粒径に選択することにより、極薄の金属配線層7でも低比抵抗の金属配線層7を可能にしたものである。 The metal wiring layer 7 containing copper as a main component can obtain a low specific resistance of 2.5 μΩcm or less even in a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm. In the formation of the copper wiring layer using the neutral electroless plating bath in which the cobalt salt is reduced, the crystal orientation of the copper plating layer depends on the crystal orientation of the metal seed layer 4 and the film of the metal wiring layer 7 The inventors have found that when the thickness is as thin as about 300 nm, the average crystal grain size of the copper plating layer is almost equal to that of the metal seed layer 4. That is, by selecting the crystal grain size of the metal seed layer 4 to be a crystal grain size for obtaining a low specific resistance of 2.5 μΩcm or less, a metal wiring layer 7 having a low specific resistance can be formed even with an extremely thin metal wiring layer 7. It is a thing.

2.5μΩcm以下の低比抵抗な無電解銅めっき配線層の形成は、大きな結晶粒径の配線層を形成することである。液晶表示装置のような表示装置の製造方法では、金属配線前後の凹凸や配線形成後の絶縁層のカバレッジ性、基板表面凹凸の低減要求等から配線厚を厚くすることで結晶粒径を大きくすることはできない。この課題を解決するために鋭意開発した結果、特に金属シード層4の結晶粒径を大きくすることにより低抵抗の銅めっき配線層が得られることを見出したものである。即ち、サブμmオーダの薄膜で2.5μΩcm以下の低比抵抗を得るためには、金属シード層4の結晶粒径を平均結晶粒径が0.25μm以上にすることにより銅めっき配線層の結晶粒径を大きくできることが判った。銅めっき配線層の結晶粒径を大きくできることは、低抵抗の銅めっき配線層を得ることができることである。このようにサブμmオーダの薄膜で、2.5μΩcm以下の低比抵抗の銅めっき層を得るためには、銅シード層の結晶性が重要であることが判った。 Formation of a low specific resistance electroless copper-plated wiring layer of 2.5 μΩcm or less is to form a wiring layer having a large crystal grain size. In the manufacturing method of a display device such as a liquid crystal display device, the crystal grain size is increased by increasing the wiring thickness due to the unevenness before and after the metal wiring, the coverage of the insulating layer after the wiring is formed, and the demand for reducing the surface unevenness of the substrate. It is not possible. As a result of diligent development to solve this problem, it has been found that a low-resistance copper-plated wiring layer can be obtained particularly by increasing the crystal grain size of the metal seed layer 4. That is, in order to obtain a low specific resistance of 2.5 μΩcm or less with a thin film on the order of sub-μm, the crystal grain size of the metal seed layer 4 is set to an average crystal grain size of 0.25 μm or more so that the crystal of the copper plated wiring layer is crystallized. It was found that the particle size can be increased. The fact that the crystal grain size of the copper-plated wiring layer can be increased is that a low-resistance copper-plated wiring layer can be obtained. Thus, it was found that the crystallinity of the copper seed layer is important in order to obtain a copper plating layer having a low specific resistance of 2.5 μΩcm or less with a thin film of the order of sub μm.

次に、金属シード層4として銅シード層と、この銅シード層上に形成される金属配線層7として銅めっき層を形成したときの、銅めっき層の平均結晶粒径とその比抵抗の具体的実施例を表1に示す。表1において、銅シード層A、B、C、Dは、共に結晶方位が主として(111)である。表1には、銅シード層の平均結晶粒径と銅シード層上に銅めっき層を無電解めっきして形成したときの、この銅めっき層の平均結晶粒径と比抵抗の関係が示めされている。   Next, when the copper seed layer is formed as the metal seed layer 4 and the copper plating layer is formed as the metal wiring layer 7 formed on the copper seed layer, the average crystal grain size of the copper plating layer and the specific resistance thereof are concretely shown. Specific examples are shown in Table 1. In Table 1, the copper seed layers A, B, C, and D all have a crystal orientation of mainly (111). Table 1 shows the relationship between the average crystal grain size of the copper seed layer and the average crystal grain size of the copper plating layer and the specific resistance when the copper plating layer is formed on the copper seed layer by electroless plating. Has been.

ここで、表1の比抵抗値は、下地金属層3及び金属シード層4を除いた金属配線層7としての銅めっき層のみの比抵抗値である。銅シード層Aは、TiNからなる下地金属層の上に形成したものであり、この銅シード層Aの平均結晶粒径は0.166μmである。この銅シード層A上に無電解めっきで形成した銅めっき層の平均結晶粒径は0.160μmである。 Here, the specific resistance values in Table 1 are specific resistance values of only the copper plating layer as the metal wiring layer 7 excluding the base metal layer 3 and the metal seed layer 4. The copper seed layer A is formed on a base metal layer made of TiN, and the average crystal grain size of the copper seed layer A is 0.166 μm. The average crystal grain size of the copper plating layer formed by electroless plating on the copper seed layer A is 0.160 μm.

銅シード層BとCは、Taからなる下地金属層の上に形成した銅シード層であり、この銅シード層BとCの平均結晶粒径は0.284μmと0.462μmである。この銅シード層BとC上に無電解めっきで形成した銅めっき層の平均結晶粒径は、それぞれ0.298μmと0.456μmである。 The copper seed layers B and C are copper seed layers formed on a base metal layer made of Ta, and the average crystal grain sizes of the copper seed layers B and C are 0.284 μm and 0.462 μm. The average crystal grain sizes of the copper plating layers formed by electroless plating on the copper seed layers B and C are 0.298 μm and 0.456 μm, respectively.

銅シード層Dは、TaSiNからなる下地金属層の上に形成したものであり、この銅シード層Dの平均結晶粒径は0.425μmである。この銅シード層D上に無電解めっきで形成した銅めっき層の平均結晶粒径は0.394μmである。 The copper seed layer D is formed on a base metal layer made of TaSiN, and the average crystal grain size of the copper seed layer D is 0.425 μm. The average crystal grain size of the copper plating layer formed by electroless plating on the copper seed layer D is 0.394 μm.

表1から判るように、下地の銅シード層の平均結晶粒径と銅めっき層の平均粒径とは、略同等であり、銅シード層の平均結晶粒径が大きい方が銅めっき層の比抵抗は、低いことが判る。即ち、比抵抗の低い銅めっき層を成膜するためには、銅シード層の平均結晶粒径を大きくすればよいことが判る。換言すれば、所望する比抵抗の銅配線層を得るためには、平均結晶粒径が相当する大きさの銅シード層を形成することにより得ることができる。主として(111)とは、X線回折により検出される(111)ピークが(200)ピークよりも大きいことを意味し、望ましくはその強度比I(111)/I(200)が10以上であることが望ましい。 As can be seen from Table 1, the average crystal grain size of the underlying copper seed layer and the average grain size of the copper plating layer are substantially the same, and the larger the average crystal grain size of the copper seed layer is, the higher the ratio of the copper plating layer. It can be seen that the resistance is low. That is, it can be seen that in order to form a copper plating layer having a low specific resistance, the average crystal grain size of the copper seed layer should be increased. In other words, in order to obtain a copper wiring layer having a desired specific resistance, it can be obtained by forming a copper seed layer having a size corresponding to the average crystal grain size. Mainly (111) means that the (111) peak detected by X-ray diffraction is larger than the (200) peak, and the intensity ratio I (111) / I (200) is preferably 10 or more. It is desirable.

比抵抗が2.2μΩcm以下の銅めっき層を得るためには、銅シード層の平均結晶粒径を略0.25μm以上にする必要がある。ここで、平均結晶粒径は、電子後方散乱(EBSP)法を用いて結晶方位が(111)の銅シード層に対して60°の双晶境界を除外して求めた値である。そして、平均結晶粒径は、結晶粒の面積から球形近似により求めた直径の平均値である。 In order to obtain a copper plating layer having a specific resistance of 2.2 μΩcm or less, the average crystal grain size of the copper seed layer needs to be about 0.25 μm or more. Here, the average crystal grain size is a value obtained by excluding a twin boundary of 60 ° with respect to a copper seed layer having a crystal orientation of (111) using an electron backscattering (EBSP) method. The average crystal grain size is an average value of diameters obtained by spherical approximation from the crystal grain area.

Figure 2006024754
Figure 2006024754

上記実施形態によれば、金属シード層の平均結晶粒径の大きな層上に金属配線層を成膜することにより平均結晶粒径の大きな金属配線層を成膜することができ、電極や配線の所望する比抵抗を得ることができる。さらに、金属配線層7は、フォトレジスト膜7に形成された溝パターン6に形成される。従って、この実施形態によれば、必要最小量の金属配線材料ですみ、省資源対応となっている。 According to the above embodiment, a metal wiring layer having a large average crystal grain size can be formed by forming a metal wiring layer on the metal seed layer having a large average crystal grain size. A desired specific resistance can be obtained. Further, the metal wiring layer 7 is formed in the groove pattern 6 formed in the photoresist film 7. Therefore, according to this embodiment, only a necessary minimum amount of metal wiring material is required and resource saving is achieved.

次に、結晶粒径が大きな金属シード層を成膜する実施形態を説明する。金属シード層として銅シード層の例について説明する。表1の銅シード層Aは、窒化チタン(TiN)層の上に銅シード層形成し、銅シード層B及び銅シード層CはTa層の上に銅シード層を形成したが、銅シード層Cの方のTa層はα-Taを主とするものである。銅シード層DはTaSiN層の上に銅シード層を形成した。銅シード層の結晶方位が主として(111)への結晶配向性や平均結晶粒径拡大のための下地金属層3としては、TiN層よりもTa系層を用いることが望ましい、Ta層及びTaSiN層の上に形成した銅シード層の方が平均結晶粒径大きくなる。Ta層においても(200)正方β−Ta層より(110)体心立方α−Ta層であることが望ましく、TaNもしくはTaN層とα−Ta層の積層膜を用いてもよい。TaN層とα−Ta層の積層膜は、Ta層のみを成膜するとβ−Ta層が形成されやすいが、Ta層の下にTaN層を薄く形成するとα−Ta層が形成されやすく、このα−Ta層上に形成される銅シード層の結晶配向性が良くなることに加え、α−Ta層の比抵抗値がβ−Ta層の比抵抗値の約1/10という利点があるためである。   Next, an embodiment in which a metal seed layer having a large crystal grain size is formed will be described. An example of a copper seed layer as a metal seed layer will be described. The copper seed layer A in Table 1 was formed by forming a copper seed layer on a titanium nitride (TiN) layer, and the copper seed layer B and the copper seed layer C were formed by forming a copper seed layer on the Ta layer. The Ta layer of C is mainly composed of α-Ta. For the copper seed layer D, a copper seed layer was formed on the TaSiN layer. It is desirable to use a Ta-based layer rather than a TiN layer as the base metal layer 3 for the crystal orientation of the copper seed layer mainly to (111) and the expansion of the average crystal grain size. Ta layer and TaSiN layer The copper seed layer formed thereon has a larger average grain size. The Ta layer is also preferably a (110) body-centered cubic α-Ta layer rather than a (200) square β-Ta layer, and a TaN layer or a stacked film of a TaN layer and an α-Ta layer may be used. The stacked film of TaN layer and α-Ta layer is likely to form a β-Ta layer if only the Ta layer is formed. However, if a thin TaN layer is formed under the Ta layer, an α-Ta layer is likely to be formed. In addition to improving the crystal orientation of the copper seed layer formed on the α-Ta layer, there is an advantage that the specific resistance value of the α-Ta layer is about 1/10 of the specific resistance value of the β-Ta layer. It is.

次に、結晶粒径が大きな金属シード層を成膜する他の実施形態を説明する。金属シード層として銅シード層の例について説明する。銅シード層の結晶粒径の拡大は、上記した下地金属層3の材質だけでなく、銅シード層を形成後、加熱処理することにより結晶粒径を拡大することができる。この加熱処理は、銅シード層を形成後、気密容器例えば真空中にて温度例えば400℃で時間例えば10分間加熱(アニール)処理することにより銅シード層の平均結晶粒径を拡大することができる。この平均結晶粒径が拡大された銅シード層上にめっきされた銅めっき層の平均結晶粒径は大きく、比抵抗は小さかった。   Next, another embodiment for forming a metal seed layer having a large crystal grain size will be described. An example of a copper seed layer as a metal seed layer will be described. The crystal grain size of the copper seed layer can be increased not only by the material of the base metal layer 3 described above but also by heat treatment after forming the copper seed layer. In this heat treatment, after the copper seed layer is formed, the average crystal grain size of the copper seed layer can be increased by heating (annealing) at a temperature, eg, 400 ° C., for a time, eg, 10 minutes, in an airtight container, eg, vacuum. . The copper plating layer plated on the copper seed layer with an enlarged average crystal grain size had a large average crystal grain size and a small specific resistance.

この加熱処理においても、下地金属層3としては、TaもしくはTa系合金を用いた方がTiNよりも銅シード層の凝集が生じにくいこともあり望ましい。   Also in this heat treatment, it is desirable to use Ta or a Ta-based alloy as the base metal layer 3 because the copper seed layer is less likely to aggregate than TiN.

次に、結晶粒径が大きな金属配線層5を成膜する他の実施形態を説明する。金属配線層5として銅めっき層の例について説明する。銅めっき層の結晶粒径の拡大は、銅シード層上に銅めっき層を形成した後に、加熱処理することで平均結晶粒径を拡大させ、比抵抗を低減することも可能である。平均結晶粒径の異なる銅シードAとBを用いて、この銅シードAとB上に形成した銅めっき層を、加熱(アニール)温度例えば450℃、加熱時間例えば10分気密雰囲気例えば真空中で加熱処理した。   Next, another embodiment for forming the metal wiring layer 5 having a large crystal grain size will be described. An example of a copper plating layer as the metal wiring layer 5 will be described. The crystal grain size of the copper plating layer can be increased by forming the copper plating layer on the copper seed layer and then heat-treating to increase the average crystal grain size and reducing the specific resistance. Using copper seeds A and B having different average crystal grain sizes, a copper plating layer formed on the copper seeds A and B is heated (annealed) at a temperature of, for example, 450 ° C. for a heating time of, for example, 10 minutes in an airtight atmosphere, for example, in a vacuum. Heat-treated.

この加熱処理後の結果は、表1に示すように結晶粒径は、拡大し、比抵抗値は低下した。例えば、銅シード層Aの上に形成した銅めっき層の平均結晶粒径は、0.160μmからアニール後0.343μmに拡大し、比抵抗値はアニール後2.53μΩcmから2.1μΩcmに低減した。銅シード層Bの上に形成した銅めっき層の平均結晶粒径は、0.298μmからアニール後0.506μmに拡大し、比抵抗値は2.18μΩcmから1.96μΩcmに低減した。銅シード層Cの上に形成した銅めっき層の平均結晶粒径は、0.456μmからアニール後0.616μmに拡大し、比抵抗値は1.97μΩcmからアニール後1.88μΩcmに低減した。銅シード層Dの上に形成した銅めっき層の平均結晶粒径は、0.394μmからアニール後0.555μmに拡大し、比抵抗値は1.99μΩcmからアニール後1.92μΩcmに低減した。 As a result after this heat treatment, as shown in Table 1, the crystal grain size increased and the specific resistance value decreased. For example, the average crystal grain size of the copper plating layer formed on the copper seed layer A increased from 0.160 μm to 0.343 μm after annealing, and the specific resistance value decreased from 2.53 μΩcm to 2.1 μΩcm after annealing. . The average crystal grain size of the copper plating layer formed on the copper seed layer B increased from 0.298 μm to 0.506 μm after annealing, and the specific resistance value decreased from 2.18 μΩcm to 1.96 μΩcm. The average crystal grain size of the copper plating layer formed on the copper seed layer C increased from 0.456 μm to 0.616 μm after annealing, and the specific resistance value decreased from 1.97 μΩcm to 1.88 μΩcm after annealing. The average crystal grain size of the copper plating layer formed on the copper seed layer D increased from 0.394 μm to 0.555 μm after annealing, and the specific resistance value decreased from 1.99 μΩcm to 1.92 μΩcm after annealing.

このように銅シード層の上に形成した各銅めっき層の平均結晶粒径は、加熱処理により拡大し、比抵抗値は低減した。ここで、加熱処理しても平均結晶粒径の大きな銅シード層の上に形成した銅めっき層の方が、平均結晶粒径は大きく、比抵抗値は小さくなった。このような結果から、平均結晶粒径が大きいめっき層の比抵抗値は小さいことが判った。 Thus, the average crystal grain size of each copper plating layer formed on the copper seed layer was increased by heat treatment, and the specific resistance value was reduced. Here, the copper plating layer formed on the copper seed layer having a large average crystal grain size even with the heat treatment had a larger average crystal grain size and a smaller specific resistance value. From these results, it was found that the specific resistance value of the plating layer having a large average crystal grain size was small.

このようにして形成された銅めっき層の平均結晶粒径と比抵抗の関係は、比抵抗増大の主要因が結晶粒界での散乱によるとする以下のモデル式を用い、反射係数R=0.58とするとよく一致することが判った。
比抵抗 ρ=ρo(バルク比抵抗)+ρGrain boundary = ρo (1+3α/2)
α=(λ/G)・R/(1−R) λ:Mean Free Path (39.3nm)
R:Reflection Coefficient (0.58) G : 結晶粒径 d:膜厚
ρo = 1.67μΩcm
The relationship between the average crystal grain size and the specific resistance of the copper plating layer formed in this way is based on the following model formula in which the main factor of the increase in specific resistance is due to scattering at the grain boundary, and the reflection coefficient R = 0.58. It was found that the results agree well.
Specific resistance ρ = ρo (bulk specific resistance) + ρGrain boundary = ρo (1 + 3α / 2)
α = (λ / G) · R / (1-R) λ: Mean Free Path (39.3nm)
R: Reflection Coefficient (0.58) G: Crystal grain size d: Film thickness
ρo = 1.67μΩcm

図3は、銅めっき層の粒界散乱モデルの上記式から求めた比抵抗と平均結晶粒径との関係を示す特性曲線と銅めっき層の実測値をプロットしたものである。この実測値は、無電解により銅めっき層を形成した後の特性(黒色)と、アニール処理後の特性(白色)とがプロットされている。図3には、上記式から求めた特性曲線がプロットされている。即ち、上記式から求めた特性曲線は、実測値の傾向とよく一致していることが示されている。図3には、無電解により銅めっき層を形成した後の特性(黒色)の4つの実施形態が、黒四角、黒丸、黒三角、黒菱形でプロットされている。これら4つの実施形態のサンプルについてアニール処理後の特性(白色)が、夫々白四角、白丸、白三角、白菱形でプロットされている。即ち、図3には、アニールすることにより平均結晶粒径が大きくなり、低比抵抗特性が得られることが示されている。   FIG. 3 is a plot of the characteristic curve showing the relationship between the specific resistance obtained from the above equation of the grain boundary scattering model of the copper plating layer and the average crystal grain size, and the measured value of the copper plating layer. In this actual measurement value, the characteristic after the copper plating layer is formed by electroless (black) and the characteristic after annealing (white) are plotted. In FIG. 3, the characteristic curve obtained from the above equation is plotted. That is, it is shown that the characteristic curve obtained from the above equation is in good agreement with the tendency of the actual measurement value. In FIG. 3, four embodiments of the characteristics (black) after the electroless copper plating layer is formed are plotted as black squares, black circles, black triangles, and black rhombuses. The characteristics (white) after annealing of the samples of these four embodiments are plotted as white squares, white circles, white triangles, and white rhombuses, respectively. That is, FIG. 3 shows that by annealing, the average crystal grain size becomes large and low specific resistance characteristics can be obtained.

図3から明らかなように、平均結晶粒径の大きな銅めっき層は、低比抵抗特性を示すことが判る。さらに、銅めっき層は、アニールすると銅めっき層の平均結晶粒径が大きくなるため、さらに、低比抵抗特性が得られることが判る。図3に示す特性曲線において、比抵抗2.2μΩcmの銅めっき層の平均結晶粒径は、0.25μmである。換え言すれば、比抵抗2.2μΩcm以下の銅めっき層を得るためには、平均結晶粒径が0.25μm以上の銅シード層を用いればよいことが判る。   As is clear from FIG. 3, it can be seen that the copper plating layer having a large average crystal grain size exhibits low specific resistance characteristics. Furthermore, it can be seen that when the copper plating layer is annealed, the average crystal grain size of the copper plating layer becomes large, and therefore, low specific resistance characteristics can be obtained. In the characteristic curve shown in FIG. 3, the average crystal grain size of the copper plating layer having a specific resistance of 2.2 μΩcm is 0.25 μm. In other words, in order to obtain a copper plating layer having a specific resistance of 2.2 μΩcm or less, it is understood that a copper seed layer having an average crystal grain size of 0.25 μm or more may be used.

しかしながら、アニールによる平均結晶粒径の拡大は、大きな結晶粒間に挟まれている小さな結晶粒が減少することが主であること、そして、銅シード層の平均結晶粒径と銅めっき層の平均結晶粒径が略等しいことから無電解めっき法による薄膜成長は、銅シード層の結晶粒上に成長した銅配線層の結晶粒がぶつかり合って膜形成が行われているものと考えられる。このことが、図3に示す特性曲線の反射係数Rは0.58と大きいことにも影響していると推測される。以上のことからも、低比抵抗値の銅配線層を無電解めっき法で形成する場合、銅シード層の結晶性や平均結晶粒径を制御することが重要であることが分かった。 However, the expansion of the average crystal grain size by annealing is mainly due to the decrease of small crystal grains sandwiched between large crystal grains, and the average crystal grain size of the copper seed layer and the average of the copper plating layer Since the crystal grain sizes are substantially equal, it is considered that the thin film growth by the electroless plating method is performed by colliding with the crystal grains of the copper wiring layer grown on the crystal grains of the copper seed layer. It is presumed that this influences that the reflection coefficient R of the characteristic curve shown in FIG. 3 is as large as 0.58. From the above, it was found that it is important to control the crystallinity and average crystal grain size of the copper seed layer when forming a copper wiring layer having a low specific resistance value by electroless plating.

上記実施形態によれば、下地金属層3の材料の選択、金属シード層4の平均結晶粒径の
大きな層、金属配線層7の平均結晶粒の大きな層にすることにより膜厚がサブμmオーダでも所望する低比抵抗の電極や配線を得ることができる。上記実施形態の金属配線層7は、配線膜厚が200〜1000nm程度のサブμmオーダの薄膜でも2.5μΩcm以下の低比抵抗(低抵抗銅配線)を得ることができる。
According to the above embodiment, the material thickness of the base metal layer 3 is selected, the metal seed layer 4 has a large average crystal grain size, and the metal wiring layer 7 has a large average crystal grain size, so that the film thickness is on the order of sub-μm. However, it is possible to obtain a desired low resistivity electrode or wiring. The metal wiring layer 7 of the above embodiment can obtain a low specific resistance (low resistance copper wiring) of 2.5 μΩcm or less even in a sub-μm order thin film having a wiring film thickness of about 200 to 1000 nm.

尚、この実施形態の配線層は、LCDだけではなく、有機EL表示装置(OLED)例えば、アクティブマトリックス型有機OLEDの基板上に形成される信号線、電源線、走査線及びTFT内の電極、及び周辺配線や同一基板上に形成された周辺駆動回路内の配線等に適用することも容易にできる。   In addition, the wiring layer of this embodiment is not only an LCD, but also an organic EL display device (OLED), for example, a signal line, a power line, a scanning line, and an electrode in a TFT formed on a substrate of an active matrix type organic OLED, In addition, the present invention can be easily applied to peripheral wiring and wiring in a peripheral driving circuit formed on the same substrate.

この実施形態の配線層の形成方法によれば、選択的に銅を主成分とする金属配線を形成でき、更に周辺駆動回路の配線に要求されるような微細配線パターンの形成が可能となる。
この実施形態の配線層は、機能素子間を電気的に接続する配線と、機能素子例えば薄膜トランシスタの電極端子とは、電気的信号の電流路である点で類似しているため、この明細書では、双方を含んで配線層と定義する。
According to the wiring layer forming method of this embodiment, a metal wiring mainly composed of copper can be selectively formed, and a fine wiring pattern as required for the wiring of the peripheral drive circuit can be formed.
The wiring layer of this embodiment is similar in that the wiring for electrically connecting the functional elements and the electrode terminal of the functional element, for example, the thin film transistor, are similar to the current signal path. Then, it defines as a wiring layer including both.

次に、上記銅めっき配線層を適用した薄膜トランジスタ回路の実施例を説明する。先ず、任意の基板に薄膜トランジスタを構成できる結晶化半導体膜の製造方法を説明する。この製造方法は、1又は複数個の薄膜トランジスタの少なくともチャネル領域を形成できる大きなシリコン結晶化領域を形成する結晶化方法について図4を参照して説明する。図4は、結晶化装置を説明するための構成図である。   Next, an embodiment of a thin film transistor circuit to which the copper plated wiring layer is applied will be described. First, a method for manufacturing a crystallized semiconductor film capable of forming a thin film transistor on an arbitrary substrate will be described. In this manufacturing method, a crystallization method for forming a large silicon crystallization region capable of forming at least a channel region of one or a plurality of thin film transistors will be described with reference to FIG. FIG. 4 is a configuration diagram for explaining the crystallization apparatus.

最小光強度が溶融温度以上の結晶化エネルギーを出力するレーザ光源10例えば紫外域の波長で例えば308nmの波長を有するXeC1エキシマレーザ光源を設ける。このレーザ光源10の光路には、入射レーザ光の光強度の均一化を行うためのホモジナイザ11が設けられる。ホモジナイザ11は、入射したレーザ光を水平方向に広げ線状(例えば、線長さ200mm)のレーザビームにし、光強度分布を均一にする装置である。ホモジナイザ11は、たとえば、複数のX方向シリンドリカルレンズをY方向に並べ、Y方向に並んだ複数の光束を形成し、他のX方向シリンドリカルレンズで各光束を再分布させ、同様複数のY方向シリンドリカルレンズをX方向に並べ、X方向に並んだ複数の光束を形成し、他のY方向シリンドリカルレンズで各光束を再分布させる光学系である。   A laser light source 10 that outputs crystallization energy having a minimum light intensity equal to or higher than the melting temperature, for example, an XeC1 excimer laser light source having a wavelength in the ultraviolet region, for example, 308 nm is provided. The optical path of the laser light source 10 is provided with a homogenizer 11 for making the light intensity of the incident laser light uniform. The homogenizer 11 is a device that spreads incident laser light in a horizontal direction to form a linear (for example, a line length of 200 mm) laser beam, and makes the light intensity distribution uniform. For example, the homogenizer 11 arranges a plurality of X-direction cylindrical lenses in the Y direction, forms a plurality of light beams arranged in the Y direction, redistributes each light beam with another X-direction cylindrical lens, and similarly, a plurality of Y-direction cylindrical lenses. This is an optical system in which lenses are arranged in the X direction, a plurality of light beams arranged in the X direction are formed, and each light beam is redistributed by another Y-direction cylindrical lens.

このホモジナイザ11の出射光路には、入射レーザ光を位相変調することにより光強度の傾斜を形成するための位相シフタ12が設けられる。光強度の傾斜は、逆ピーク状の光強度最小分布の光ビームであり、連続する略三角形状の光強度分布を有し、最小光強度が溶融温度以上のエネルギー光である。位相シフタ12は、例えば石英基材に段差をつけ、段差の境界でレーザ光の回折と干渉を起こさせ、レーザ光強度に周期的な空間分布を付与するものである。位相シフタ12は、例えば段差部x=0を境界として左右で180度の位相差を付けた場合である。一般にレーザ光の波長をλとすると、屈折率nの透明媒質を透明基材上に形成して180度の位相差を付けるには、透明媒質の膜厚tは、t=λ/2(n−1)で与えられる。石英基材の屈折率を1.46とすると、XeC1エキシマレーザ光の波長が308nmであるから、180度の位相差を付けるためには334.8nmの段差をエッチング等の方法でつければよい。またSiN膜を透明媒質としてPECVD、LPCVD等で成膜する場合は、SiN膜の屈折率を2.0とすると、SiN膜を石英基材上に154nm成膜し、エッチングして段差を付ければ良い。180度の位相をつけた位相シフトマスクを通過したレーザ光の強度は、周期的強弱のパターンを示す。 In the outgoing optical path of the homogenizer 11, a phase shifter 12 is provided for forming a light intensity gradient by phase-modulating the incident laser light. The light intensity gradient is a light beam with an inverse peak-shaped light intensity minimum distribution, a continuous light intensity distribution having a substantially triangular shape, and energy light whose minimum light intensity is equal to or higher than the melting temperature. For example, the phase shifter 12 is provided with a step in a quartz base material, causes diffraction and interference of laser light at the step boundary, and gives a periodic spatial distribution to the laser light intensity. The phase shifter 12 is a case where a phase difference of 180 degrees is given on the left and right, for example, with the stepped portion x = 0 as a boundary. In general, when the wavelength of the laser beam is λ, a transparent medium having a refractive index n is formed on a transparent substrate to give a phase difference of 180 degrees. The film thickness t of the transparent medium is t = λ / 2 (n -1). If the refractive index of the quartz substrate is 1.46, the wavelength of the XeC1 excimer laser light is 308 nm. Therefore, in order to add a phase difference of 180 degrees, a step of 334.8 nm may be formed by a method such as etching. When the SiN x film is formed as a transparent medium by PECVD, LPCVD, etc., if the refractive index of the SiN x film is 2.0, the SiN x film is formed on the quartz substrate at 154 nm and etched to form a step. You can add. The intensity of the laser light that has passed through the phase shift mask having a phase of 180 degrees shows a pattern of periodic strength.

この位相シフタ12の出射光路には、位相シフタ12で形成された光強度分布を結像するための結像光学系13が設けられる。この結像光学系13の結像位置には、被結晶化基板14が設けられる。この被結晶化基板14は、X・Y・Z・θステージ(図示せず)上に、位置合わせして設けられる。このステージは、予め記憶されたプログラムにより被結晶化基板14の予め定められた位置に自動的に結晶化操作が行われるように移動する。このようにして結晶化装置15が構成されている。結晶化操作とは、大きさ例えば1m角の被結晶化基板14のどこの位置に結晶化のためのレーザ光を照射するかの情報が予め記憶されたプログラムによりステージを順次移動させて、レーザ光を照射させる制御をいう。 An imaging optical system 13 for forming an image of the light intensity distribution formed by the phase shifter 12 is provided in the outgoing optical path of the phase shifter 12. A crystallized substrate 14 is provided at the imaging position of the imaging optical system 13. The crystallized substrate 14 is provided in alignment on an X · Y · Z · θ stage (not shown). This stage moves so that the crystallization operation is automatically performed at a predetermined position on the crystallized substrate 14 by a program stored in advance. In this way, the crystallization apparatus 15 is configured. The crystallization operation means that the stage is sequentially moved by a program in which information on which position of the crystallized substrate 14 having a size of, for example, 1 m square is irradiated with laser light for crystallization is stored in advance. Control that emits light.

この結晶化装置15による結晶化は、ローダに設けられた被結晶化基板14をステージの予め定められた位置に、位置合わせして搬送し、微細位置合わせしたのち、レーザ光源10を照射制御することにより、自動的に被結晶化基板14が結晶化される。即ち、レーザ光源10を操作してパルスレーザ光を出射させる。このパルスレーザ光は、ホモジナイザ11に入射して光強度分布の均一化および位相シフタ12への入射角の均一化が行われる。   In the crystallization by the crystallization apparatus 15, the substrate 14 to be crystallized provided in the loader is aligned and transported to a predetermined position on the stage, finely aligned, and then the laser light source 10 is controlled to be irradiated. As a result, the crystallized substrate 14 is automatically crystallized. That is, the laser light source 10 is operated to emit pulsed laser light. This pulsed laser light is incident on the homogenizer 11 to make the light intensity distribution uniform and make the incident angle to the phase shifter 12 uniform.

ホモジナイザ11で均一化されたレーザ光は、位相シフタ12に入射して位相変調され、光強度の傾斜した光強度分布に変調される。位相変調されたレーザ光は、結像光学系13により集光されて被結晶化基板14に入射する。このレーザ光は、被結晶化基板14に入射して非単結晶半導体膜の照射領域を溶融する。パルス期間が、終了し、レーザ光の被結晶化基板14への入射が遮断されると、溶融領域は、急速に降温する。この降温過程において、光強度分布の傾斜に沿って固液分岐点の通過に応じて結晶化が横方向に行われる。この横方向の結晶化が長く続くように被結晶化基板14は、次のような構造になっている。   The laser beam made uniform by the homogenizer 11 is incident on the phase shifter 12 and is phase-modulated to be modulated into a light intensity distribution with a light intensity gradient. The phase-modulated laser light is collected by the imaging optical system 13 and enters the crystallized substrate 14. This laser light is incident on the crystallized substrate 14 and melts the irradiation region of the non-single crystal semiconductor film. When the pulse period ends and the incidence of laser light on the crystallized substrate 14 is interrupted, the temperature of the melted region rapidly decreases. In this temperature lowering process, crystallization is performed in the lateral direction according to the passage of the solid-liquid branch point along the slope of the light intensity distribution. The crystallized substrate 14 has the following structure so that the lateral crystallization continues for a long time.

基板例えばガラス基板21上には、この基板21からの不純物浸透の防止およびレーザ光に照射されて溶融したときの温度を蓄熱する機能を有する絶縁体層例えば酸化シリコン膜22を設けられている。この酸化シリコン膜22上には、非単結晶半導体膜例えば非晶質半導体膜23が設けられている。この非晶質半導体膜23上には、レーザ光に照射されて溶融したときの温度を蓄熱する機能を有するキャップ膜例えば酸化シリコン膜24を設けられている。このような積層構造により被結晶化基板14が構成されている。   On a substrate such as a glass substrate 21, an insulator layer such as a silicon oxide film 22 is provided which has a function of preventing impurities from penetrating from the substrate 21 and storing the temperature when melted by irradiation with laser light. On the silicon oxide film 22, a non-single crystal semiconductor film such as an amorphous semiconductor film 23 is provided. On the amorphous semiconductor film 23, a cap film, for example, a silicon oxide film 24 having a function of storing a temperature when melted by irradiation with laser light is provided. The crystallized substrate 14 is configured by such a laminated structure.

この被結晶化基板14に上記パルスレーザ光が入射したときパルスレーザ光は、酸化シリコン膜24を透過して非晶質半導体膜23に吸収される。非晶質半導体膜23のパルスレーザ光の受光領域は、融点以上の高温度に瞬時に上昇し、瞬時に溶融する。この高温度の熱は、非晶質半導体膜23の表裏面に設けられている酸化シリコン膜22および24に蓄熱される。入射パルスレーザの入射が遮断されたとき、非晶質半導体膜23の溶融領域は、高速に降温しようとするが、表裏面の酸化シリコン膜22および24の蓄熱により降温速度が緩やかな降温となり、光強度の傾斜にならって結晶化が進み、横方向に大粒径の結晶化領域が形成される。大粒径の結晶化領域は、1又は複数個の薄膜トランジスタからなる薄膜トランジスタ回路の形成を可能にする。   When the pulse laser light is incident on the crystallized substrate 14, the pulse laser light passes through the silicon oxide film 24 and is absorbed by the amorphous semiconductor film 23. The light-receiving area of the pulsed laser beam in the amorphous semiconductor film 23 instantaneously rises to a temperature higher than the melting point and melts instantly. This high temperature heat is stored in the silicon oxide films 22 and 24 provided on the front and back surfaces of the amorphous semiconductor film 23. When the incidence of the incident pulse laser is cut off, the melted region of the amorphous semiconductor film 23 tries to cool down at a high speed, but the temperature drop rate is lowered slowly due to the heat accumulation of the silicon oxide films 22 and 24 on the front and back surfaces. Crystallization proceeds along with the gradient of light intensity, and a crystallized region having a large grain size is formed in the lateral direction. The large grain size crystallization region allows the formation of a thin film transistor circuit consisting of one or more thin film transistors.

この結晶化プロセスは、ステージを移動させ、レーザ光のショットを繰り返することにより被結晶化基板14の広い範囲に結晶化領域を形成することを可能にする。 This crystallization process makes it possible to form a crystallization region in a wide range of the crystallized substrate 14 by moving the stage and repeating the shot of laser light.

次に、上記大粒径の結晶化領域に薄膜トランジスタ回路を形成した実施形態を図5を参照して説明する。図4と同一部分には、同一符号を付与し、その詳細な説明を省略する。図5は、非晶質半導体膜23に形成された大粒径の結晶化領域に位置合わせして形成した薄膜トランジスタ回路31を示す断面図である。   Next, an embodiment in which a thin film transistor circuit is formed in the large grain size crystallization region will be described with reference to FIG. The same parts as those in FIG. 4 are denoted by the same reference numerals, and detailed description thereof is omitted. FIG. 5 is a cross-sectional view showing a thin film transistor circuit 31 formed in alignment with a large grain size crystallization region formed in the amorphous semiconductor film 23.

薄膜トランジスタ回路は、図4の結晶化装置15により結晶化された被結晶化基板14の結晶化領域に形成される。この被結晶化基板14の表面に形成されている酸化シリコン膜24は、除去して用いられ、この状態が図5に示されている。   The thin film transistor circuit is formed in the crystallization region of the crystallized substrate 14 crystallized by the crystallization apparatus 15 of FIG. The silicon oxide film 24 formed on the surface of the crystallized substrate 14 is removed and used, and this state is shown in FIG.

非晶質半導体膜23の結晶化領域30には、ソース領域32、ドレイン領域33およびチャネル領域34が設けられている。このソース領域32およびドレイン領域33間の上記結晶化領域表面上には、ゲート絶縁膜35例えば酸化シリコン膜が成膜されている。この酸化シリコン膜上でソース領域32およびドレイン領域33間上方には、ゲート電極36が設けられている。このゲート電極36およびゲート絶縁膜35上には、層間絶縁膜37として窒化シリコン膜38と酸化シリコン膜39と窒化シリコン膜40とが積層成膜されている(積層構造は図示せず)。   A source region 32, a drain region 33, and a channel region 34 are provided in the crystallization region 30 of the amorphous semiconductor film 23. On the surface of the crystallization region between the source region 32 and the drain region 33, a gate insulating film 35 such as a silicon oxide film is formed. On the silicon oxide film, a gate electrode 36 is provided above the source region 32 and the drain region 33. On the gate electrode 36 and the gate insulating film 35, a silicon nitride film 38, a silicon oxide film 39, and a silicon nitride film 40 are stacked as an interlayer insulating film 37 (the stacked structure is not shown).

ソース領域32とドレイン領域33の電極を形成するために層間絶縁膜37には、コンタクトホールが穿設されている。各コンタクトホールには、ソース電極42およびドレイン電極43が埋設されている。ソース電極42およびドレイン電極43上には窒化シリコンからなるパシベーション層44が設けられている。上記の層間絶縁膜37の中の窒化シリコン膜38、窒化シリコン膜39及び窒化シリコンからなるパシベーション層40は、銅拡散のバリア層としても機能している。また、ゲート絶縁膜35は、酸化シリコン膜の
単層よりも銅拡散のバリア性を有する窒化シリコン膜との積層構造とする方が低抵抗配線層を形成する面から望ましい。
In order to form the electrodes of the source region 32 and the drain region 33, a contact hole is formed in the interlayer insulating film 37. A source electrode 42 and a drain electrode 43 are embedded in each contact hole. A passivation layer 44 made of silicon nitride is provided on the source electrode 42 and the drain electrode 43. The passivation layer 40 made of the silicon nitride film 38, the silicon nitride film 39, and the silicon nitride in the interlayer insulating film 37 also functions as a copper diffusion barrier layer. The gate insulating film 35 is preferably laminated with a silicon nitride film having a barrier property of copper diffusion rather than a single layer of silicon oxide film from the viewpoint of forming a low resistance wiring layer.

上記ゲート電極36、ソース電極42、ドレイン電極43には、本実施形態の配線層が適用されている。この配線については、図1および図2と同一部分には、同一符号を付与し、その詳細な説明は、重複するので省略する。   The wiring layer of this embodiment is applied to the gate electrode 36, the source electrode 42, and the drain electrode 43. In this wiring, the same parts as those in FIGS. 1 and 2 are denoted by the same reference numerals, and detailed description thereof will be omitted because it is duplicated.

すなわち、ゲート電極36、ソース電極42およびドレイン電極43は、いずれも下地金属層3を形成し、この下地金属層3上に金属シード層4を形成し、この金属シード層4上に金属配線層7を形成した構成である。ゲート電極36は、ゲート絶縁膜35上に下地金属層3を成膜し、続いて金属シード層4、金属配線層7を成膜した後、パターンニングすることにより形成することができる。   That is, the gate electrode 36, the source electrode 42, and the drain electrode 43 all form the base metal layer 3, the metal seed layer 4 is formed on the base metal layer 3, and the metal wiring layer is formed on the metal seed layer 4. 7 is formed. The gate electrode 36 can be formed by depositing the base metal layer 3 on the gate insulating film 35, subsequently forming the metal seed layer 4 and the metal wiring layer 7, and then patterning.

ソース電極42およびドレイン電極43は、夫々ソース領域32およびドレイン領域33上に位置合わせして形成されたコンタクトホール内に下地金属層3を埋設し、続いて金属シード層4、金属配線層7を成膜して形成することができる。ここで、ゲート電極36、ソース電極42およびドレイン電極43を構成する銅配線層の上にはバリア性を有する窒化シリコン膜が積層されているが、窒化シリコン膜に加えて少なくとも金属シード層4、金属配線層7の露出している表面を例えばCoWB、CoBやCoWP、CoPのようなバリア性を有する合金層で予め無電解めっき法によって覆うようにしてもよいことは言うまでもない。 In the source electrode 42 and the drain electrode 43, the base metal layer 3 is embedded in contact holes formed in alignment on the source region 32 and the drain region 33, respectively, and then the metal seed layer 4 and the metal wiring layer 7 are formed. It can be formed by film formation. Here, a silicon nitride film having a barrier property is laminated on the copper wiring layer constituting the gate electrode 36, the source electrode 42, and the drain electrode 43. However, in addition to the silicon nitride film, at least the metal seed layer 4, Needless to say, the exposed surface of the metal wiring layer 7 may be covered in advance by an electroless plating method with an alloy layer having a barrier property such as CoWB, CoB, CoWP, or CoP.

このようにして図5に示すように薄膜トランジスタ回路31を形成することができる。この薄膜トランジスタ回路31は、液晶表示装置や有機EL表示装置の製造を可能にする。 Thus, the thin film transistor circuit 31 can be formed as shown in FIG. The thin film transistor circuit 31 enables manufacture of a liquid crystal display device or an organic EL display device.

以上説明したように上記実施形態によれば、膜厚がサブμmオーダで比抵抗が2.5μΩcm以下の低抵抗銅配線を可能にすることができる。特に、薄膜トランジスタや薄膜トランジスタ回路を構成することができる。   As described above, according to the above embodiment, a low resistance copper wiring having a film thickness on the order of sub-μm and a specific resistance of 2.5 μΩcm or less can be realized. In particular, a thin film transistor or a thin film transistor circuit can be formed.

本発明方法の実施形態で配線までの中間工程を工程順に説明するための断面図である。It is sectional drawing for demonstrating the intermediate process to wiring in order of process in embodiment of this invention method. 図1の工程の次の配線工程を工程順に説明するための断面図である。FIG. 2 is a cross-sectional view for explaining a wiring process subsequent to the process of FIG. 図2の工程で得られた配線の平均結晶粒径に対する比抵抗の関係を示す特性曲線図である。It is a characteristic curve figure which shows the relationship of the specific resistance with respect to the average crystal grain diameter of the wiring obtained at the process of FIG. 図2の低抵抗配線を薄膜トランジスタ回路に適用した実施形態を説明するための結晶化装置説明図である。FIG. 3 is an explanatory diagram of a crystallization apparatus for explaining an embodiment in which the low resistance wiring of FIG. 2 is applied to a thin film transistor circuit. 図4の結晶化装置により製造された結晶化領域に形成された薄膜トランジスタ回路の構成を具体的に説明するための断面図である。FIG. 5 is a cross-sectional view for specifically explaining a configuration of a thin film transistor circuit formed in a crystallization region manufactured by the crystallization apparatus of FIG. 4.

符号の説明Explanation of symbols

1:ガラス基板、 2:下地絶縁層、 3:下地金属層、 4:金属シード層、
5:フォトレジスト層、 6:溝パターン、 7:金属配線層、 14:被結晶化基板、 15:結晶化装置、 21:ガラス基板、 22,24:酸化シリコン膜、
23:非晶質半導体膜、 30:結晶化領域、 31:薄膜トランジスタ回路、
32:ソース領域、 33ドレイン領域、 35:ゲート絶縁膜、36:ゲート電極、 37:層間絶縁膜、 42:ソース電極、 43:ドレイン電極、 44:パシベーション層。
1: glass substrate, 2: underlying insulating layer, 3: underlying metal layer, 4: metal seed layer,
5: Photoresist layer, 6: Groove pattern, 7: Metal wiring layer, 14: Substrate to be crystallized, 15: Crystallizer, 21: Glass substrate, 22, 24: Silicon oxide film,
23: Amorphous semiconductor film, 30: Crystallized region, 31: Thin film transistor circuit,
32: source region, 33 drain region, 35: gate insulating film, 36: gate electrode, 37: interlayer insulating film, 42: source electrode, 43: drain electrode, 44: passivation layer.

Claims (12)

主結晶面が(111)で、平均結晶粒径が0.25μm以上の金属シード層を形成する工程と、
前記金属シード層上に膜厚が200乃至1000nmの金属配線層を無電解めっきする工程と
を具備してなることを特徴とする配線層の形成方法。
Forming a metal seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more;
And a step of electroless plating a metal wiring layer having a thickness of 200 to 1000 nm on the metal seed layer.
主結晶面が(111)で、平均結晶粒径が0.25μm以上の銅シード層を形成する工程と、
前記銅シード層上に膜厚が200乃至1000nmの銅配線層を無電解めっきする工程と
を具備してなることを特徴とする配線層の形成方法。
Forming a copper seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more;
And a step of electrolessly plating a copper wiring layer having a thickness of 200 to 1000 nm on the copper seed layer.
基板上に下地金属層を形成する工程と、
前記下地金属層上に主結晶面が(111)で、平均結晶粒径が0.25μm以上の銅シード層を形成する工程と、
前記銅シード層上に膜厚が200乃至1000nmで予め定められたパターンの銅配線層を無電解めっきする工程と、
少なくとも前記銅配線層と接合される領域以外の前記銅シード層および前記下地金属層を除去する工程と
を具備してなることを特徴とする配線層を形成する方法。
Forming a base metal layer on the substrate;
Forming a copper seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more on the underlying metal layer;
Electroless plating a copper wiring layer having a predetermined pattern with a film thickness of 200 to 1000 nm on the copper seed layer;
A method of forming a wiring layer, comprising: removing at least the copper seed layer and the base metal layer other than a region bonded to the copper wiring layer.
前記無電解めっき液は、コバルト塩を還元剤とするアルカリ金属フリーの中性無電解めっき浴であることを特徴とする請求項1乃至3のいずれか1項記載の配線層の形成方法。 4. The method of forming a wiring layer according to claim 1, wherein the electroless plating solution is an alkali metal-free neutral electroless plating bath using a cobalt salt as a reducing agent. 前記シード層は、スパッタリングにより形成された膜であることを特徴とする請求項1乃至3のいずれか1項記載の配線層の形成方法。   4. The method for forming a wiring layer according to claim 1, wherein the seed layer is a film formed by sputtering. 前記配線層は、エピタキシャル成長した層であることを特徴とする請求項1乃至3のいずれか1項記載の配線層の形成方法。   4. The method for forming a wiring layer according to claim 1, wherein the wiring layer is an epitaxially grown layer. 前記シード層および前記配線層は、350℃以上の温度でアニール処理された層であることを特徴とする請求項1乃至5のいずれか1項記載の配線層の形成方法。   6. The method of forming a wiring layer according to claim 1, wherein the seed layer and the wiring layer are layers annealed at a temperature of 350 ° C. or higher. 金属シード層上に金属配線層が設けられた配線層であって、前記金属シード層は結晶面が(111)で、平均結晶粒径が0.25μm以上であり、前記金属配線層は膜厚が200乃至1000nmであり、無電解めっきされた層であることを特徴とする配線層。 A wiring layer provided with a metal wiring layer on a metal seed layer, wherein the metal seed layer has a crystal plane of (111) and an average crystal grain size of 0.25 μm or more, and the metal wiring layer has a film thickness A wiring layer having a thickness of 200 to 1000 nm and an electroless plated layer. 銅シード層上に銅配線層が設けられた配線層であって、前記銅シード層と銅配線層の平均結晶粒径は略同じ大きさであることを特徴とする配線層。 A wiring layer in which a copper wiring layer is provided on a copper seed layer, wherein the copper seed layer and the copper wiring layer have substantially the same average grain size. 前記銅シード層の下地には、Ta,β−Ta,α−Ta,TaSiN,TaN,TaNとα−Taの積層膜のうち少なくも一つの材料層により構成されていることを特徴とする請求項9記載の配線層。 The underlayer of the copper seed layer is composed of at least one material layer of a stacked film of Ta, β-Ta, α-Ta, TaSiN, TaN, TaN, and α-Ta. Item 10. The wiring layer according to Item 9. 前記銅シード層の平均結晶粒径は、0.25μm以上であることを特徴とする請求項9又は10記載の配線層。 11. The wiring layer according to claim 9, wherein an average crystal grain size of the copper seed layer is 0.25 μm or more. 結晶化領域を有する半導体薄膜と、
前記結晶化領域内にソース領域およびドレイン領域が設けられ、前記結晶化領域にゲート絶縁膜を介して設けられたゲート電極を有する薄膜トランジスタとを具備し、
前記薄膜トランジスタのソース電極、ドレイン電極、ゲート電極の少なくとも1つの電極は主結晶面が(111)で、平均結晶粒径が0.25μm以上の金属シード層と、この金属シード層上に設けられた膜厚が200乃至1000nmの無電解めっき層とで構成したものであることを特徴とする薄膜トランジスタ。
A semiconductor thin film having a crystallized region;
A source region and a drain region are provided in the crystallization region, and a thin film transistor having a gate electrode provided in the crystallization region via a gate insulating film,
At least one of the source electrode, the drain electrode, and the gate electrode of the thin film transistor is provided on a metal seed layer having a main crystal plane of (111) and an average crystal grain size of 0.25 μm or more, and the metal seed layer. A thin film transistor comprising an electroless plating layer having a thickness of 200 to 1000 nm.
JP2004201683A 2004-07-08 2004-07-08 Wiring layer, forming method thereof, and thin-film transistor Pending JP2006024754A (en)