CS199323B1 - Process for preparing magnesium oxide from dolomites and dolomite calcites - Google Patents

Process for preparing magnesium oxide from dolomites and dolomite calcites Download PDF

Info

Publication number
CS199323B1
CS199323B1 CS132679A CS132679A CS199323B1 CS 199323 B1 CS199323 B1 CS 199323B1 CS 132679 A CS132679 A CS 132679A CS 132679 A CS132679 A CS 132679A CS 199323 B1 CS199323 B1 CS 199323B1
Authority
CS
Czechoslovakia
Prior art keywords
magnesium
magnesium oxide
dolomite
leaching
ammonium
Prior art date
Application number
CS132679A
Other languages
Czech (cs)
Slovak (sk)
Inventor
Ivan Novak
Jan Petrovic
Original Assignee
Ivan Novak
Jan Petrovic
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ivan Novak, Jan Petrovic filed Critical Ivan Novak
Priority to CS132679A priority Critical patent/CS199323B1/en
Publication of CS199323B1 publication Critical patent/CS199323B1/en

Description

(54) Spfisob výroby kysličníka horečnatého z dolomitov a dolomitických vápencov(54) Method of production of magnesium oxide from dolomites and dolomitic limestones

Vynález rieši spfisob výroby kysličníka horečnatého z dolomitov a dolomitických vápencov.SUMMARY OF THE INVENTION The present invention provides a method for producing magnesium oxide from dolomite and dolomite limestone.

Základnou surovinou pre výrobu žiaruvzdorných magnezitových ma teriálov je magnezit, MgCOy V surovom magnezite sú okrem uhličitanu horečnatého ako akcesorie obyčejné přítomné aj variabilně množstvá kysličníka křemičitého, kysličníka hlinitého, kysličníka vápenatého a hlavně kysličníka železitého. PokiaT sú v magnezite tieto příměsi přítomné len v obmedzenom malom množstve, ovplyvňujú konečné vlastnosti žiaromateriálov len poměrně málo.The basic raw material for the production of refractory magnesite materials is magnesite, MgCOy In addition to magnesium carbonate, magnesite, as well as the usual magnesium oxide, alumina, alumina, calcium oxide and mainly iron oxide are present in the raw magnesite. As long as these impurities are present in a limited small amount in magnesite, they affect the final properties of the refractory materials only relatively little.

V dfisledku pokračujúceho vyčerpávania zdrojov kvalitných magnezitov a tým núteného přechodu na neustále menej hodnotné suroviny sa však stává čorraz obtiažnejšie udržiavať kvalitu žiarovýrobkov na žiadúcej úrovni. Preto je nutné v stále širšom měřítku postupné prikročovať k fyzikálnym a najmS chemickým spfisobom obohacovania surového magnezitu. Ide hlavně o odatraňovanie vysokých podielov kysličníka křemičitého a najma kysličníka železitého ·However, due to the continuing depletion of sources of high-quality magnesia and the forced transition to ever-less valuable raw materials, it becomes more difficult to maintain the quality of the refractory products at the desired level. Therefore, it is necessary to gradually and gradually proceed to the physical and especially chemical methods of enrichment of crude magnesite. It is mainly about the removal of high proportions of silica and especially iron oxide.

V poslednej době sa pri výrobě žiaromateriálov na báze kysličníka horečnatého začína uplatňovat nový trend priamej výroby z čistého kysličníka horečnatého, připravovaného chemickou cestou. Tak napr. sú vypracované epfieoby výroby magnézia z mořskéj vody, kde v morskej vodě přítomný chlorid horečnatý sa zráža pomocou hydroxidu vápenatého na hydroxid horěčnatý. Nevýhodou tohto spfisobu výroby kysličníka horečnatého je značné nízká koneentrácia východiskového chloridu horečnatého a problémy s neželate&iou koprecipitáciou niektorýchRecently, a new trend of direct production from pure magnesium oxide prepared by chemical processes has begun to be applied in the production of magnesium oxide-based materials. So eg. Magnesia production from seawater has been elaborated where magnesium chloride present in seawater precipitates with calcium hydroxide to magnesium hydroxide. The disadvantage of this method of magnesium oxide production is the considerable low concentration of the starting magnesium chloride and the problems of unwanted coprecipitation of some

199Ό23199Ό23

199 323 dalších kysličníkov, v mořskéj vodě přítomných (napr. kysličník boritý).199,323 other oxides present in seawater (eg boric oxide).

Preto vfičáina navrhovaných metod výroby čistého kysličníka horečnatého vychádza zo aurového magnezitu, ktorý sa obyčajne z dóvodov zníženia rozpustnosti kysličníka železitého kalcinuje na teploty 1100-1200 °C, načo aa takto vypálený magnezit rozpúšťa v kyselinách. Ak ea k rozpúěťaniu používá kyselina dusičná, prevádza sa vzniknutý duáičnan horečnatý zrážaním pomocou kvapalného amoniaku na hydroxid horečnatý. Při použití kyseliny chlorovodíkovej ako rozpúšťadla, sa vzniknutý roztok chloridu horečnatého po zahuštění rozetrekuje v reaktoři pri 600 °C, kde se Stiepi priamo na kysličník horečnatý a chlorovctdík.Therefore, most of the proposed methods for producing pure magnesium oxide are based on auric magnesite, which is usually calcined at temperatures of 1100-1200 ° C to reduce the solubility of ferric oxide, and then dissolves magnesite in acids. When nitric acid is used for dissolution, the resulting magnesium dilate is converted to magnesium hydroxide by precipitation with liquid ammonia. When using hydrochloric acid as the solvent, the resulting magnesium chloride solution is thickened in the reactor at 600 ° C, where it is cleaved directly onto magnesium oxide and hydrogen chloride.

Existuje tiež spósob bikarbonátový, kde ea suspenzia sýti pri chladení s kysličníkom uhličitým a vzniknutý rozpustný hydrouhličitan horečnatý sa pri zvýšenej teplote rozkládá na nerozpustný trihydrát uhličitanu horečnatého.There is also a bicarbonate process wherein ea suspension is carbonated on cooling with carbon dioxide and the resulting soluble magnesium bicarbonate decomposes at elevated temperature to insoluble magnesium carbonate trihydrate.

Nedostatky týchto spósobov sú - okrem dosť komplikovanéj technologie a nevyrieáenosti problémov v oblasti konátrukčných materiálov - hlavně v znečisťovaní životného prostredia a v potiažach s využitím odpadových produktov.The deficiencies of these methods are - in addition to the rather complicated technology and unresolved problems in the field of construction materials - mainly in environmental pollution and in the problems of using waste products.

Nedávno boli opísané spósoby výroby zásaditého uhličitanu horečnatého selektívnym lúžením vyčíhaného magnezitu vodnými roztokmi amonných solí niektorých organických kyselin, s výhodou mravčenov a oxalátov amonných:. Z roztoku mravčanu amonného sa po odstránení nerozpustných nečistót vyzráža zásaditý uhličitan horečnatý vháňaním amoniaku a kysličníka uhličitého.Recently, processes for the production of basic magnesium carbonate by selective leaching of spent magnesite with aqueous solutions of ammonium salts of some organic acids, preferably formates and ammonium oxalates have been described. The basic magnesium carbonate precipitates from the ammonium formate solution after removal of the insoluble impurities by injecting ammonia and carbon dioxide.

Existuje aj spósob výroby kysličníka horečnatého z dolomitu; tak například sa podlá rumunského patentu č. 59 712 připravuje kysličník horečnatý dvojstupňovou úpravou dolomitu: v 1. stupni sa vypálený dolomit upravuje odpadnými roztokmi z amoniakového spósobu výroby e<3dy, pričom vzniká hydroxid horečnatý; v druhom stupni se tento Salčj upravuje prídavkom odpadových roztokov, čím vzniká roztok chloridu horečnatého, ktorý sa po zbavení chloridu vápenatého zráža hydrouhličitanom sodným, čím vzniká uhličitan horečnatý, ktorý vyčíháním dává kysličník horečnatý.There is also a method of producing magnesium oxide from dolomite; for example, according to Romanian patent no. 59 712 prepares magnesium oxide by a two-stage treatment of dolomite: in the first stage, the fired dolomite is treated with waste solutions from the ammonia production process e <3dy to form magnesium hydroxide; in the second step, this salc is treated by adding waste solutions to form a magnesium chloride solution which precipitates upon removal of the calcium chloride by sodium bicarbonate, thereby forming magnesium carbonate, which gives magnesium oxide by leaching.

Iný spósob popísáný v rumunskom patente č. 59 779 spočívá v tom, že sa dolomit upravuje roztokmi, odpadajúcimi pri výrobě sody amoniakovým spdsobom, načo sa získaný roztok saturuje kyaličníkom uhličitým, načo po filtrácii a oddělení poeledných zvyškov chloridu vápenatého pomocou uhličitanu horečnatého, sa roztok chloridu horečnatého upravuje hydrouhličitanom sodným pri 25 °C, čím vzniká uhličitan horečnatý.Another method described in Romanian patent no. 59 779 consists of treating dolomite with ammonia-free solutions of soda water, saturating the resulting solution with carbon tetrachloride, and after filtering and separating the traces of calcium chloride with magnesium carbonate, the magnesium chloride solution is treated with sodium bicarbonate at 25 ° C to form magnesium carbonate.

Vyššie uvedené nedostatky nemá spósob výroby kysličníka horečnatého z dolomitov a dolomitických vápencov podlá vynálezu, ktorého podstata spočívá v tom, že dolomit alebo dolomitický vápenec, s výhodou vo formě dolomitických pieskov, připadne odpadných dolomitických prachov a kusových dolomitov sa podrobí selektívnej kalcinácii pri teplotách od 650 °C do 850 °C, načo sa vyžíhaný produkt podrobí vyluhovaniu roztokmi, s výhodou 10 - 40 % vodnými roztokmi, amonných solí anorganických kyselin, s výhodou síranu a) alebo dusičnanu a) alebo chloridu amonného, obsahujúcich amónnu soT v množstve 100 až 200 molárnych %, vztiahnu tých na obsah kysličníka horečnatého v polovypálenom dolomite, pričom vyluhováni® sa robí pri teplote 50 až 110 °C po dobu 5 až 20 minút, e výhodou 5 až 10 minút, načo při použitíThe above-mentioned drawbacks have no method for producing magnesium oxide from dolomites and dolomitic limestones according to the invention, which consists in that dolomite or dolomitic limestone, preferably in the form of dolomitic sands, or waste dolomitic powders and lump dolomites is subjected to selective calcination at temperatures from 650 ° C to 850 ° C, whereupon the annealed product is leached with solutions, preferably 10-40% aqueous solutions, of ammonium salts of inorganic acids, preferably of sulphate a) or of nitrate a) or of ammonium chloride containing an ammonium salt of 100 to 200 mole%, based on the magnesium oxide content of the semi-calcined dolomite, the leaching being carried out at a temperature of 50 to 110 ° C for 5 to 20 minutes, preferably 5 to 10 minutes, where in use

199 323 síranu amonného k vyluhovaniu polovypáleného dolomitu sa po vyluhovaní a oddělení tuhej fázy podrobí.zíakaný roztok kryštalizácii, s výhodou ochladením horúceho roztoku pod 5 °C, načo ea vykrystalizovaný síran horečnatý po vyaušení rozloží kalcináciou při teplote v rozmedzí 1000 až 1200 °C na kysličník horečnatý, lebo pri použití síranu a) alebo dusičnanu a) alebo chloridu amonného k vylučovaniu sa po vyluhovaní a oddělení tuhej fázy zo získaného roztoku horečnatej soli zráža zásaditý uhličitan horečnatý pomocou súčasného alebo za sebou privádzaného amoniaku a kysličníka uhličitého, načo sa tento po oddělení a vysušení kalcinuje pri teplote nad 400 °C na kysličník horečnatý, alebo na výluh zráža kysélinou oxalovou alebo oxalátom amonným na oxalát horečnatý, ktorý po oddělení od matočného lúhu sa podrobí kalcinácii pri teplote nad 550 °C na kysličník horečnatý.After leaching and separating the solid phase, 199 323 ammonium sulphate for leaching semi-calcined dolomite is subjected to crystallization, preferably by cooling the hot solution below 5 ° C, after which the crystallized magnesium sulphate after decomposition is decomposed by calcination at a temperature of 1000 to 1200 ° C. magnesium oxide, because with the use of sulphate a) or nitrate a) or ammonium chloride to precipitate, after leaching and separation of the solid phase, the basic magnesium carbonate precipitates from the obtained magnesium salt solution with simultaneous or successive ammonia and carbon dioxide. and drying calcines at a temperature above 400 ° C for magnesium oxide, or precipitates on the leachate oxalic acid or ammonium oxalate to magnesium oxalate, which after separation from the mother liquor is subjected to calcination at a temperature above 550 ° C to magnesium oxide.

Selektívna kalcinácia sa prevádza tak, aby všetok v dolomite obsiahnutý uhličitan horečnatý prešiel na MgO a CaCO^ ostal nerozložený.Selective calcination is carried out so that all of the dolomite contained magnesium carbonate is converted to MgO and CaCO2 remains decomposed.

Výhodou spčsobu výroby kysličníka horečnatého podl’a vynálezu je, že rieši výrobu kysličníka horečnatého najmfi využíváním podřadných alebo odpadových karbonátových surovin obsahujúcich hořčík. S výhodou je možno k výrobě použiť piesčité dolomity, ktoré hoci chemicky velmi čisté, eú nevhodné pre vfičšinu aplikácii z hlediska svojej eypkosti. Ďalej možno takto spracovávať odpady, vznikajúce pri úpravě vysokohodnotných dolomitov.An advantage of the process for producing magnesium oxide according to the invention is that it solves the production of magnesium oxide by using, in particular, inferior or waste magnesium-containing carbonate raw materials. Advantageously, sand dolomites may be used which, although chemically very pure, are unsuitable for most applications in terms of their euphony. Furthermore, waste resulting from the treatment of high-value dolomites can be treated in this way.

Materiál ostávajúci po vyluhovaní kysličníka horečnatého představuje v podstatě čistý uhličitan vápenatý, ktorý možno využiť ako plnohodnotná surovinu (výroba cement, slinku, v sklárstve a pod.). V tejto súvislosti možno uvažovať o využití vynálezu k odstraňovaniu vyšších obsahov kysličníka horečnatého z vápencov tam, kde je přítomnost kysličníka horečnatého nežiadúca ^kysličník vápenatý pre stavebníctvo, výroba cementu, lahké stavebné hmoty, at3.).The material remaining after the leaching of magnesium oxide is essentially pure calcium carbonate, which can be used as a full-value raw material (cement, clinker, glass, etc.). In this context, consideration may be given to using the invention to remove higher levels of magnesium oxide from limestone where the presence of magnesium oxide is undesirable calcium oxide for construction, cement production, lightweight building materials, etc.).

Příklad 1Example 1

Vypálením 5 kg dolomitu pri teplote 825 °C sa získal polovypálený dolomit s obsahom 27,21 % kysličníka horečnatého. Takto získaný materiál sa pomlel a preosial sitom 0,5 mm.The burning of 5 kg of dolomite at 825 ° C resulted in semi-fired dolomite containing 27.21% magnesium oxide. The material so obtained was ground and sieved through a 0.5 mm screen.

Příklad 2Example 2

Vždy po 100 g polovypáleného dolomitu připraveného podlá příkladu 1 sa podrobilo vyluhovaniu v 230 ml 40 % roztoku síranu amonného po dobu 5 min pri teplote 100 °C, načo po odfiltrovaní a premytí sa v matečnom výluhu analyticky stanovil obsah kysličníka horečnatého a kysličníka vápenatého. V tabulke 1 sú uvedené výsledky pre příslušné teploty a doby vyluhovania.In each case 100 g of semi-baked dolomite prepared according to Example 1 were subjected to leaching in 230 ml of a 40% ammonium sulfate solution for 5 min at 100 [deg.] C., after filtration and washing, the magnesium and calcium oxides were analyzed analytically in the mother liquor. Table 1 shows the results for the respective temperatures and leaching times.

Tabulka 1Table 1

Teplota vyluhovanía Extraction temperature 100 °C Mp 100 ° C 90 °C 90 ° C 70 °0 70 ° 0 doba vyluhovania (min) leaching time (min) 5 5 10 10 20 20 5 5 10 10 20 20 5 5 10 10 20 20 obsah MgO vo výluhu, na polovypál.dolom. (%) MgO content in the leachate, on a semi-burnt mine. (%) 26,75 26.75 26,94 26.94 27,02 27,02 26,19 26.19 26,82 26.82 26,94 26.94 25,05 25.05 26,32 26,32 26,74 26.74 obsah CaO vo výluhu, na polovypál.dolom. (%) CaO content in the leachate, in a semi-burnt mine. (%) 1,00 1.00 2,14 2.14 6,16 6.16 0,85 0.85 1,17 1.17 2,47 2.47 0,75 0.75 1,10 1.10 1,74 1.74

199 323199 323

Příklad 3Example 3

100 g polovypáleného dolomitu připraveného podl’a příkladu 1 sa podrobilo vyluhovaniu v 230 ml 40 % roztoku síranu amonného po dobu 20 minút pri teplote 70 °C. Ďalej sa postupovalo ako v příklade 2.100 g of semi-baked dolomite prepared according to Example 1 was subjected to leaching in 230 ml of a 40% ammonium sulfate solution for 20 minutes at 70 ° C. The procedure was as in Example 2.

Příklad 4Example 4

100 g polovypáleného dolomitu připraveného podlá příkladu 1 se podrobilo vyluhovaniu v 230 ml 40 % roztoku síranu amonného po dobu 10 minút při teplote 90 °C. Ďalej sa postupovalo eko v příklade 2.100 g of semi-fired dolomite prepared according to Example 1 were subjected to leaching in 230 ml of a 40% ammonium sulfate solution for 10 minutes at 90 ° C. The eco procedure of Example 2 was then followed.

Příklad 5Example 5

Vždy po 100 g polovypáleného dolomitu připraveného podlá příkladu 1 se podrobilo vyluhovaniu v 1 li tri 10 % roztoku síranu amonného po dobu 5 minút pri teplote 100 °C, načo po odfiltrovaní a premytí sa vo výluhu stanovil analyticky obsah kysličníka horečnatého a kysličníka vápenatého. V tabulke 2 sú výsledky uvedené pre příslušné teploty a doby vyluhovania.In each case 100 g of semi-fired dolomite prepared according to Example 1 were subjected to leaching in 1 l of a 10% ammonium sulfate solution for 5 minutes at 100 ° C, after which the magnesium oxide and calcium oxide were analyzed analytically in the extract. Table 2 shows the results for the respective leaching temperatures and times.

Tabulka 2Table 2

-y η----- Teplota vyluhovania -y η ----- Extraction temperature ICO °c ICO ° c 90 °C 90 ° C 70 °C 70 ° C 50 °C Deň: 32 ° C doba vyluhovaní a Ámin) leaching time and Amin) 5 5 10 10 20 20 5 5 10 10 20 20 5 5 10 10 20 20 7^ 5 7 ^ 5 10 10 20 20 obsah IčgO vo výluhu na polovyp. dol. ίίϋ the content of IgO in the leachate per half. dol. ίίϋ 25,92 25.92 26,47 26.47 26,83 26.83 24,85 24.85 25,56 25.56 26,14 26.14 25,31 25.31 25,94 25.94 26,36 26.36 19,43 19.43 22,62 22.62 23,73 23.73 obsah OaQ vo výluhu, na polovyp. dol. («) content of OaQ in the extract, per half. dol. ( «) 0,96 0.96 1,49 1.49 3,42 3.42 0,38 0.38 0,75 0.75 1,10 1.10 0,35 0.35 0,69 0.69 0,88 0.88 0,28 0.28 0,45 0.45 0,65 0.65

Příklad 6Example 6

100 g polovypáleného dolomitu připraveného podlá příkladu 1 sa podrobilo vyluhovaniu v 1 litri 10 % roztoku síranu amonného po dobu 20 minút pri teplote 50 °C.100 g of semi-fired dolomite prepared according to Example 1 were subjected to leaching in 1 liter of 10% ammonium sulfate solution for 20 minutes at 50 ° C.

Ďalej aa postupovalo ako v příklade 5.Next, aa proceeded as in Example 5.

Příklad 7Example 7

100 g polovypáleného dolomitu připraveného podle příkladu 1 aa podrobilo vyluhovaniu v 1 litri 10 % roztoku síranu amonného po dobu 10 minút při teplote 70 °C. Ďalej sa postupovalo ako v příklade 5.100 g of semi-baked dolomite prepared according to Example 1 aa was subjected to leaching in 1 liter of 10% ammonium sulfate solution for 10 minutes at 70 ° C. The procedure was as in Example 5.

Příklad 8Example 8

0,5 kg dolomitu aa kalcinuje pri teplote 690 °C, načo sa získaný materiál premelie a preoseje sitom 0,5 mm a vyluhuje v 2,5 litre 30 % roztoku dusičnanu amonného po dobu 10 min pri teplote 85 °C. Po odfiltrovaní a schladení sa na roztok p6sobí súčasne plynným amoniakom a kyaličníkom uhličitým po dobu 30 min pri prietoku každého z plynov 200 ml/min.0.5 kg of dolomite aa is calcined at 690 ° C, after which the material obtained is ground and sieved through a 0.5 mm sieve and leached in 2.5 liters of 30% ammonium nitrate solution for 10 min at 85 ° C. After filtering and cooling, the solution is treated simultaneously with ammonia gas and carbon dioxide for 30 min at a flow rate of 200 ml / min for each of the gases.

Získaná zrazenina zásaditého uhličitanu horečnatého sa oddělí od roztoku filtráciou. Vysušený materiál sa kaleinuje pri teplote 440 °C. Takto sa získalo 95 g kysličníka horečnatého, čo je zhruba 92 % výťažok z celkového obsahu kysličníka horečnatého v dolomite.The resulting precipitate of basic magnesium carbonate is separated from the solution by filtration. The dried material is calibrated at 440 ° C. This gave 95 g of magnesium oxide, which is about 92% yield of the total magnesium oxide content of dolomite.

Příklad 9Example 9

Vypálený dolomit podlá příkladu 1 o hmotnosti 0,5 kg sa podrobil vyluhovaniu v 1,75 litra 30 % roztoku síranu amo'nneho pri 90 °C po dobu 8 min. Po odfiltrovaní sa horúci roztok ochladil na 15 °C, načo po 30-minútovej kryštalizácii sa vzniknuté kryštály oddělili filtráciou. Získaný síran horečnatý sa vyčíhal pri teplote 1050 °C. Získala sa pálená magnézia s obsahom 98,60 % kysličníka horečnatého.The burned dolomite of Example 1 weighing 0.5 kg was subjected to leaching in 1.75 liters of a 30% ammonium sulfate solution at 90 ° C for 8 min. After filtration, the hot solution was cooled to 15 ° C, after crystallization for 30 minutes, the formed crystals were collected by filtration. The magnesium sulfate obtained was calcined at 1050 ° C. Burnt magnesium was obtained containing 98.60% of magnesium oxide.

Příklad 10Example 10

K 0,5 kg polovypáleného dolomitu podl’a příkladu 1 sa přidali 2 litre 20 % roztoku chloridu amonného. Vyluhovanie so vykonalo pri teplote 70 °C po dobu 10 min. Po filtrácii sa k roztoku přidalo 500 g oxalátu amonného. Po rozpuštění a prereagovaní sa získala zrazenina oxalátu horečnatého, ktorý po odfiltrovaní a premytí aa vyčíhal při teplote 600 °C. Získal sa produkt v množstve 129 g, obsahujúci 95,37 % kysličníka horečnatého.To 0.5 kg of the semi-baked dolomite of Example 1 was added 2 liters of 20% ammonium chloride solution. Extraction was carried out at 70 ° C for 10 min. After filtration, 500 g of ammonium oxalate was added to the solution. Upon dissolution and reaction, a precipitate of magnesium oxalate was obtained, which, after filtration and washing, and calcined at 600 ° C. The product was obtained in an amount of 129 g, containing 95.37% of magnesium oxide.

Claims (1)

PREDMET VYNÁLEZUOBJECT OF THE INVENTION Spdsob výroby kysličníka horečnatého z dolomitov a dolomitických vápencov vyznačujúci sa tým, že dolomit alebo dolomitický vápenec, s výhodou vo formě dolomitických pieskov, připadne odpadných dolomitických prachov a kusových dolomitov nevhodných pre iné použitie, sa podrobí selektívnej kalcinácii při teplotách od 650 °C do 850 °C, načó sa vyžíhaný produkt podrobí vyluhovaniu roztokmi, s výhodou 10 až 40 % vodnými roztokmi, amonných solí anorganických kyselin, s výhodou síranu a) alebo dusičnanu a) alebo chloridu amonného, obsahujúcich amónnu sol v množstve 100 až 200 molárnych % vztiahnutých na obsah kysličníka horečnatého v polovypálenom dolomite, pričom vyluhovanie sa robí pri teplote 50 až 110 °C po dobu 5 až 20 minút, s výhodou 5 až 10 minút, načo pri použití síranu amonného k vyluhovaniu polovypáleného dolomitu sa po vyluhovaní a oddělení tuhej fázy podrobí získaný roztok kryštalizácii, s výhodou ochladením horúceho roztoku pod 15 °C, načo sa vykrystalizovaný síran horečnatý po vysušení rozloží kalcináciou pri teplote v rozmedzí 1000 až 1200 °C na kysličník horečnatý, lebo pri použití síranu a) alebo dusičnanu a) alebo chloridu amonného k vyluhovaniu sa po vyluhovaní a oddělení tuhej fázy zo získaného roztoku horečnatej soli zráža zásaditý uhličitan horečnatý pomocou súčasného alebo za sebou privádzaného amoniaku a kysličníka uhličitého, načo sa tento po oddělení a vysušení kalcinuje pri teplote nad 400 °C na kysličník horečnatý, alebo na výluh zráža kyselinou oxalovou alebo oxalátom amonným na oxalát horečnatý, ktorý po oddělení od matočného lúhu sa podrobí kalcinácii pri teplote nad 550 °C na kysličník horečnatý.Process for producing magnesium oxide from dolomites and dolomitic limestones, characterized in that dolomite or dolomitic limestone, preferably in the form of dolomitic sands or waste dolomitic powders and lump dolomites unsuitable for other uses, is subjected to selective calcination at temperatures from 650 ° C to 850 ° C ° C, after which the annealed product is leached with solutions, preferably 10 to 40% aqueous solutions, of ammonium salts of inorganic acids, preferably of sulfate a) or of nitrate a) or of ammonium chloride, containing an ammonium salt in an amount of 100 to 200 mole% based on the magnesium oxide content of the semi-fired dolomite, the leaching being carried out at a temperature of 50 to 110 ° C for 5 to 20 minutes, preferably 5 to 10 minutes, after which the ammonium sulphate for leaching the semi-burned dolomite is subjected to solution by crystallization, preferably about cooling the hot solution below 15 ° C, whereupon the crystallized magnesium sulphate after drying is decomposed into magnesium oxide by calcination at a temperature of 1000 to 1200 ° C, because using a) or nitrate a) or ammonium chloride for leaching after leaching and separation The solid phase precipitates the basic magnesium carbonate from the obtained magnesium salt solution with simultaneous or successively introduced ammonia and carbon dioxide, which after separation and drying is calcined at a temperature above 400 ° C for magnesium oxide, or precipitated on the leach by oxalic acid or ammonium oxalate to magnesium oxalate which, after separation from the mother liquor, is subjected to calcination at a temperature above 550 ° C to produce magnesium oxide.
CS132679A 1979-02-28 1979-02-28 Process for preparing magnesium oxide from dolomites and dolomite calcites CS199323B1 (en)