CN1800462A - Method for producing spinning corduroy using multiple ingredient cotton spinning and staple wool blended yarn - Google Patents

Method for producing spinning corduroy using multiple ingredient cotton spinning and staple wool blended yarn Download PDF

Info

Publication number
CN1800462A
CN1800462A CN200610037716.4A CN200610037716A CN1800462A CN 1800462 A CN1800462 A CN 1800462A CN 200610037716 A CN200610037716 A CN 200610037716A CN 1800462 A CN1800462 A CN 1800462A
Authority
CN
China
Prior art keywords
yarn
corduroy
spinning
cotton
burner
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN200610037716.4A
Other languages
Chinese (zh)
Other versions
CN1800462B (en
Inventor
赵国瑛
张建良
张新龙
杨自治
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Heilan Home Co Ltd
Original Assignee
Sainuo Science And Technology Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sainuo Science And Technology Co Ltd filed Critical Sainuo Science And Technology Co Ltd
Priority to CN200610037716.4A priority Critical patent/CN1800462B/en
Publication of CN1800462A publication Critical patent/CN1800462A/en
Application granted granted Critical
Publication of CN1800462B publication Critical patent/CN1800462B/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to a method for using multi-component cotton yarn and staple wool blended yarn to produce fine-spinning corduroy, which comprises: a, using fine-spinning yarn as the chaine and latitude as non-cut yarn, the chaine branches as 40/2-120/2, the latitude branches as 40/2-120/2; using the blended yarn of cellulose/chappe silk yarn/cotton or cellulose/chappe/cashmere as pile-cut yarn, while the yarn branches as 30/1-60/1 or 60/2-120/2; the components comprises: cotton in 45-55 deals, cellulose in 35-45 deals, the chappe in 3-8 deals, or chappe in 65-75 deals, cellulose in 20-25 deals, and cotton in 3-8 deals; the rate between latitude tension degree and chaine tension degree is 2-3:1; b, the edge organism is corduroy smooth edge, as 12 upper, 12 or 13 upper and 23 lower square organism; c, the surface of coiling shaft is grain surface or seta surface; d, after-cleaning uses burning genappe on the corduroy fabric, the temperature is 600-900Deg. C, the speed is 60-80m/min, and the distance between fabric and burner is 30-80mm; e, first wetting and cutting in the after-cleaning process: genapping, washing, crabbing and drying. The invention has high density, smooth surface and soft feeling.

Description

Many components cotton spun yarn and combing wool blended yarn are produced the method for spinning corduroy
Technical field:
The present invention relates to a kind of production method of spinning corduroy, especially relate to the method that a kind of model, spun silk, cotton, cashmere cotton spun yarn, wool, blend polyester spun yarn are produced spinning corduroy.
Background technology:
Traditional corduroy goods are raw materials used to be Quality Pure Cotton Yarn Production or line mostly, the part kind adopts and to wash/and silk/cotton blended yarn, spun rayon or cotton fiber/height contraction acrylic blended yarn.With the corduroy fabric of these raw material production have that feel is abundant, the suede bar is mellow and full, lines is clear, the plentiful characteristics such as concordant of fine hair, but also exist shortcomings such as drapability is poor, gloss deficiency, outward appearance low grade.
For addressing the above problem, ZL02157297.6 discloses a kind of hair corduroy, and its raw material adopts wool fibre and silk blending yarn as velvet-pile yarn, promptly as the pile filling of corduroy; The ground weft of non-velvet-pile yarn adopts wool fibre/terylene mixed yarn in its raw material, and warp thread adopts the pure wool yarn, and the fabric ground tissue of corduroy adopts the plain weave alternative construction.This hair corduroy makes the premium properties of wool fibre and spun silk well be brought into play on quality, both embodied wear-resisting, the strong characteristics of traditional cotton corduroy fabric, and made it obtain soft gloss and good drapability, wrinkle resistance, gas permeability and hygroscopicity again.Product gloss is soft, nature, style are rough bold and unconstrained, and ABRASION RESISTANCE is not well lost the body bone of wool fabric again.But it still has the some shortcomings part:
1, density is low, and finished product fabric fine hair is not plentiful, easily balling-up and take off seam.
2, the limit is organized as burr, corduroy dyes, puts in order after generally adopting grey cloth cylinder gassing frame to singe, as above-mentioned technology is used in the wool fibre is on the corduroy of raw material, can cause that then coloured light changes a lot, and wool fibre is produced very big damage, as without singing, the finished product corduroy then has irregular long toe feathering and reverse side hair phenomenon.
3, the back arrangement adopts first clipping rewetting whole, is on the corduroy of raw material as above-mentioned technology is used in the wool fibre, and the finished product fabric easily produces wrinkle and cuts defect, and feel is not ideal.
Summary of the invention:
The objective of the invention is to overcome above-mentioned deficiency, the method that provides a kind of density height, smooth surface, soft many components cotton spun yarn and combing wool blended yarn to produce spinning corduroy.
The object of the present invention is achieved like this: a kind of many components cotton spun yarn and combing wool blended yarn are produced the method for spinning corduroy, are characterized in:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 40/2~120/2, and ground weft is single thread or twine, and yarn count is 40/2~120/2; The blended yarn that adopts model/spun silk/cotton or model/spun silk/cashmere is as velvet-pile yarn, promptly as the Velveteen of corduroy, the Velveteen yarn count is 30/1~60/1 or 60/2~120/2, Velveteen composition weight portion is: cotton 45~55, model 35~45, spun silk 3~10, or spun silk 65~75, model 20~25, cashmere 3~10; Fabric latitude tightness be 2~3: 1 through the tightness ratio,
B, limit are organized as corduroy plain edge tissue, the limit is organized as on 12, on the 12 belows flat limit tissue or 13, flat limit, 13 belows tissue,
C, select the winding off spindle surface to be grain or thorn hair side when weaving,
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 600~900 ℃, and the speed of a motor vehicle is 60~80 meters/minute, and distance is 30~80mm between fabric and burner,
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open width is washed mud, crabbing, oven dry.
Compare with existing corduroy, the present invention has following advantage:
1, corduroy through close low, filling density is high, it is plentiful and prevent the finished product fabric pilling and become the pint seam to be beneficial to finished product fabric fine hair.
2, the limit is organized as plain edge, makes the by-pass crochet reach smooth even.
3, adopt grey cloth burner singeing, the fabric positive and negative are smooth, nothing becomes mildewed, and avoided the face hair to produce and changes of shade.
4, wet earlier whole clipping is again adopted in the back arrangement, avoids the finished product fabric folding line to be arranged, good hand touch.
Through the improvement of said method, finished product fabric of the present invention except that the superior elasticity that has kept wool, wrinkle resistance, the gloss of the softness of the cotton of holding concurrently, comfortable and model, its superior performance shows the following aspects:
1, quality in kind: fibers such as high-grade fine wool, cotton fiber, model, spun silk, cashmere combine, through deep processing, and good quality of product, the process environmental protection belongs to green product.
2, have excellent elasticity, wrinkle resistance, flexibility, comfort, gas permeability is better, and unique cashmere feel, style are arranged again.
3, compare with similar corduroy product, have ratio of performance to price height, market popularization value height, characteristics such as good in economic efficiency.
The specific embodiment:
Embodiment 1:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 40/2, and ground weft is single thread or twine, and yarn count is 40/2; The blended yarn that adopts cotton/model/spun silk is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 30/1, and suede yarn composition weight portion is: cotton/model/spun silk: 50/45/5; Fabric latitude tightness be 2: 1 through the tightness ratio.
B, limit are organized as corduroy plain edge tissue, and the limit is organized as on 12, flat limit, 12 belows tissue.
C, select the winding off spindle surface to be the thorn hair side when weaving.
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 600 ℃, and the speed of a motor vehicle is 60 meters/minute, and distance is 30mm between fabric and burner.
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open washing, crabbing, oven dry.
F, the dried whole horizontal bristle that is make fine hair hold up obvolvent.
Embodiment 2:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 60/2, and ground weft is single thread or twine, and yarn count is 60/2; The blended yarn that adopts cotton/model/spun silk is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 40/1, and suede yarn composition weight portion is: cotton/model/spun silk: 45/45/10; Fabric latitude tightness be 2.5: 1 through the tightness ratio.
B, limit are organized as corduroy plain edge tissue, and the limit is organized as on 12, flat limit, 12 belows tissue.
C, select the winding off spindle surface to be grain when weaving.
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 700 ℃, and the speed of a motor vehicle is 70 meters/minute, and distance is 50mm between fabric and burner,
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open washing, crabbing, oven dry.
F, the dried whole horizontal bristle that is make fine hair hold up obvolvent.
Embodiment 3:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 80/2, and ground weft is single thread or twine, and yarn count is 80/2; The blended yarn that adopts cotton/model/spun silk is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 60/1, and suede yarn composition weight portion is: cotton/model/spun silk: 55/40/5; Fabric latitude tightness be 2: 1 through the tightness ratio.
B, limit are organized as corduroy plain edge tissue, and the limit is organized as on 13, flat limit, 13 belows tissue.
C, select the winding off spindle surface to be grain when weaving.
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 800 ℃, and the speed of a motor vehicle is 80 meters/minute, and distance is 80mm between fabric and burner,
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open washing, crabbing, oven dry.
F, the dried whole horizontal bristle that is make fine hair hold up obvolvent.
Embodiment 4:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 100/2, and ground weft is single thread or twine, and yarn count is 100/2; The blended yarn that adopts model/spun silk/cashmere is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 60/2, and Velveteen composition weight portion is: spun silk/model/cashmere: 70/25/5; Fabric latitude tightness be 3: 1 through the tightness ratio,
B, limit are organized as corduroy plain edge tissue, and the limit is organized as on 13, flat limit, 13 belows tissue,
C, select the winding off spindle surface to be the thorn hair side when weaving,
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 900 ℃, and the speed of a motor vehicle is 75 meters/minute, and distance is 70mm between fabric and burner,
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open washing, crabbing, oven dry.
F, the dried whole horizontal bristle that is make fine hair hold up obvolvent.
Embodiment 5:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 120/2, and ground weft is single thread or twine, and yarn count is 120/2; The blended yarn that adopts model/spun silk/cashmere is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 80/2, and Velveteen composition weight portion is: spun silk/model/cashmere: 75/20/5; Fabric latitude tightness be 2.5: 1 through the tightness ratio,
B, limit are organized as corduroy plain edge tissue, and the limit is organized as on 13, flat limit, 13 belows tissue,
C, select the winding off spindle surface to be the thorn hair side when weaving,
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 800 ℃, and the speed of a motor vehicle is 75 meters/minute, and distance is 60mm between fabric and burner,
All the other are with example 4.
Embodiment 6:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 120/2, and ground weft is single thread or twine, and yarn count is 120/2; The blended yarn that adopts model/spun silk/cashmere is as velvet-pile yarn, and promptly as the Velveteen of corduroy, the Velveteen yarn count is 100/2 or 120/2, and Velveteen composition weight portion is: spun silk/model/cashmere: 75/20/5; Fabric latitude tightness with through tightness than 2.5: 1,
All the other are with example 5.

Claims (7)

1, a kind of many components cotton spun yarn and combing wool blended yarn are produced the method for spinning corduroy, it is characterized in that:
A, the spinning hair of employing are washed warp thread and the ground weft of yarn as non-velvet-pile yarn, and the warp thread yarn count of non-velvet-pile yarn is 40/2~120/2, and ground weft is single thread or twine, and yarn count is 40/2~120/2; The blended yarn that adopts model/spun silk/cotton or model/spun silk/cashmere is as velvet-pile yarn, promptly as the Velveteen of corduroy, the Velveteen yarn count is 30/1~60/1 or 60/2~120/2, Velveteen composition weight portion is: cotton 45~55, model 35~45, spun silk 3~10, or spun silk 65~75, model 20~25, cashmere 3~10; Fabric latitude tightness be 2~3: 1 through the tightness ratio,
B, limit are organized as corduroy plain edge tissue, the limit is organized as on 12, on the 12 belows flat limit tissue or 13, flat limit, 13 belows tissue,
C, select the winding off spindle surface to be grain or thorn hair side when weaving,
D, back arrangement adopt corduroy fabric grey cloth burner to singe, and the burner temperature is 600~900 ℃, and the speed of a motor vehicle is 60~80 meters/minute, and distance is 30~80mm between fabric and burner,
Wet earlier whole clipping is again adopted in e, back arrangement, and wet whole science and engineering skill is: singe, open washing, crabbing, oven dry.
2, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: the warp thread yarn count of described non-velvet-pile yarn is 40/2~40/2, and the ground weft yarn count is 40/2~60/2; The Velveteen yarn count is 30/1~50/1.
3, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: the warp thread yarn count of described non-velvet-pile yarn is 60/2~80/2, and the ground weft yarn count is 60/2~80/2; The Velveteen yarn count is 60/2~80/2.
4, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: the warp thread yarn count of described non-velvet-pile yarn is 80/2~100/2, and the ground weft yarn count is 80/2~100/2; The Velveteen yarn count is 80/2~100/2.
5, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: the warp thread yarn count of described non-velvet-pile yarn is 100/2~120/2, and the ground weft yarn count is 100/2~120/2; The Velveteen yarn count is 100/2~120/2.
6, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: described grey cloth burner is singed, and the burner temperature is 600~700 ℃, and the speed of a motor vehicle is 60~80 meters/minute, distance is 30~50mm between fabric and burner
7, produce the method for spinning corduroy according to the described a kind of many components cotton spun yarn of claim 1 and combing wool blended yarn, it is characterized in that: described grey cloth burner is singed, the burner temperature is 700~900 ℃, and the speed of a motor vehicle is 60~80 meters/minute, and distance is 50~80mm between fabric and burner.
CN200610037716.4A 2006-01-10 2006-01-10 Method for producing spinning corduroy using multiple ingredient cotton spinning and staple wool blended yarn Expired - Fee Related CN1800462B (en)