CN1586123A - Process for producing ornaments or artificial jade relief flower pot - Google Patents

Process for producing ornaments or artificial jade relief flower pot Download PDF

Info

Publication number
CN1586123A
CN1586123A CN 200410070444 CN200410070444A CN1586123A CN 1586123 A CN1586123 A CN 1586123A CN 200410070444 CN200410070444 CN 200410070444 CN 200410070444 A CN200410070444 A CN 200410070444A CN 1586123 A CN1586123 A CN 1586123A
Authority
CN
China
Prior art keywords
model
cured
mold
add
shade
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 200410070444
Other languages
Chinese (zh)
Inventor
李翠华
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 200410070444 priority Critical patent/CN1586123A/en
Publication of CN1586123A publication Critical patent/CN1586123A/en
Pending legal-status Critical Current

Abstract

The present invention features that prepared jade material is deposited into various products with enjoying, collecting and developing value. The products have short making period, low cost, fine technique, pure color, and various sizes, shapes, colors, etc.

Description

The process for making of ornaments or artificial jade relief flower pot
Technical field
The present invention relates to the making construction method of ornaments or artificial jade relief flower pot, belong to watering and mould, carve, imitate the material product field.
Existing jade is ring, Xu vessel used to hold grain at the imperial sacrifice, bracelet, and kind is single, so goods are not so good as Counterfeit Item and work with great care on sense organ, moulding and different, imitated vestige numerous in variety.
The purpose of this invention is to provide the process for making of ornaments or artificial jade relief flower pot material and goods, goods obviously are better than existing goods, and the Counterfeit Item duration is short, and cost is low; Not being subjected to the restriction in environment, space, kind, specification, color, classification, traditional handicraft, material, environmental protection, market, is to have material and the goods of viewing and admiring, collect, develop value.
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add thinner with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) the three-dimensional soft or hard mould of system:
(1) fixed model: the position that model is narrow down, wide position stands on the tabula rasa up, adds talcum powder with 502 glue, by 100: 10~30 fixed ratio;
(2) system soft mold: add with silicon rubber and to solidify Ji, mix well, water and be filled on the model, up catch up with the mixing silicon rubber that grey cutter will down drop down from the model, till solidifying by 100: 5~20 ratio mixing;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system gypsum mold: add curing agent with 801 glue, mix by 100: 50~80 ratio and mix well, be put on half of soft mold, extremely above till over half 0,5~10 centimeters of soft mold;
(5) drying: dried in the shade 5~10 minutes,
(6) remove mould: the plaster mold over half 0,5~10 centimeters above soft mold removed;
(7) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half soft mold that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(8) system hard mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the soft mold of cured half, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(9) drying: dried in the shade 10~30 minutes;
(10) remove mould: the gypsum mold of second half of the hard mold that will make is all removed, and cleans up;
(11) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the soft mold of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(12) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on the soft mold of half of removing gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(13) drying: dried in the shade 10~30 minutes;
(14) die sinking: hard mold is opened respectively, taken out soft mold, soft mold is cut a mouth, take out the model of the inside;
(15) cut edge: the burr around the hard mold are cut off,
(16) polishing: corase grind machine, correct grinding are by hand, and be extremely smooth straight and even;
(17) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of soft or hard mould, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
3) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold: silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes;
(6) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(7) upward cured; The floor is cured or mould is cured or table leather board spray is cured, brush or be sprayed on the soft or hard mould inner wall, to dry in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
4) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiber board or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
5) the imitative jade material of system: the transparent resin gel coat is added thinner add curing agent and add=100: 10~30:: 10~30.
5) imitative jade material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: the transparent resin gel coat is added thinner add curing agent, ratio mixing in 100: 10~30: 10~30 is mixed well, water with vessel and to be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, with the limit that a plurality of clips are clamped mould, above-mentioned hybrid resin can't be leached;
(3) drying: dry in the shade to just solidifying,
(4) die sinking tool: open mould, take out early-products;
(5) engraving: early-products is engraved as the goods that adhere to specification;
(6) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(7) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(8) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till satisfied;
(9) drying: dried in the shade 10~30 minutes;
(10) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
Combination shaping:
(1) main body is shaped: the goods of making by above-mentioned same process method all are combined on the main body with methods such as perforating, bonding, vertebra connect, allow body reach design standard;
(2) engraving: adhesive has been carved, cleaned up;
(3) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(4) gluing: with above-mentioned transparent hybrid resin goods are described, to the standard that adheres to specification;
(5) drying: dried in the shade 30 minutes~1 hour;
(6) drying: with being sprayed on the goods from spraying paint, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
With ornaments or the artificial jade relief flower pot that above-mentioned process for making is finished, it is exquisite, elegant in appearance to do manual work, and is that the utmost point has material and the goods of viewing and admiring, develop value.
Embodiment:
Introduce the step of making ornaments or artificial jade relief flower pot material and goods of process provided by the present invention below.
Ornaments or jade relief flower pot profile: long * wide * high=0.98 meter * 0.68 meter * 0.78 meter
Basic pattern is a relief flower pot that has two dragons to rob precious pattern.
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add thinner with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) the three-dimensional soft or hard mould of system:
(1) fixed model: the position that model is narrow down, wide position stands on the tabula rasa up, adds talcum powder with 502 glue, by 100: 10~30 fixed ratio;
(2) system soft mold: add with silicon rubber and to solidify Ji, mix well, water and be filled on the model, up catch up with the mixing silicon rubber that grey cutter will down drop down from the model, till solidifying by 100: 5~20 ratio mixing;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system gypsum mold: add curing agent with 801 glue, mix by 100: 50~80 ratio and mix well, be put on half of soft mold, extremely above till over half 0,5~10 centimeters of soft mold;
(5) drying: dried in the shade 5~10 minutes;
(6) remove mould: the plaster mold over half 0,5~10 centimeters above soft mold removed;
(7) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half soft mold that does not water gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(8) system hard mold 1: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush was being gone up on the soft mold of cured half, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(9) drying: dried in the shade 10~30 minutes;
(10) remove mould: the gypsum mold of second half of the hard mold that will make is all removed, and cleans up;
(11) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on half the soft mold of having removed gypsum mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
(12) system hard mold 2: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush is on the soft mold of half of removing gypsum mold, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed on fine glass fibre cloth, layer overlay thick glass fibre cloth is brushed above-mentioned hybrid resin on thick glass fibre cloth again;
(13) drying: dried in the shade 10~30 minutes;
(14) die sinking: hard mold is opened respectively, taken out soft mold, soft mold is cut a mouth, take out the model of the inside;
(15) cut edge: the burr around the hard mold are cut off,
(16) polishing: corase grind machine, correct grinding are by hand, and be extremely smooth straight and even;
(17) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the inwall of soft or hard mould, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
3) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold: silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes
(6) go up cured: analyse ground cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the soft or hard mould inner wall, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
4) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiber board or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
5) the imitative jade material of system: the transparent resin gel coat is added thinner add curing agent=100: 10~30: 10~30.
6) imitative jade material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: the transparent resin gel coat is added thinner add curing agent, ratio mixing in 100: 10~30: 10~30 is mixed well, water with vessel and to be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, with the limit that a plurality of clips are clamped mould, above-mentioned hybrid resin can't be leached;
(3) drying: dry in the shade to just solidifying;
(4) die sinking tool: open mould, take out early-products;
(5) engraving: early-products is engraved as the goods that adhere to specification;
(6) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(7) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(8) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till the standard that adheres to specification;
(9) drying: dried in the shade 10~30 minutes;
(11) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
Combination shaping 1:
(1) main body is shaped: by perforating bonding, joggle, grafting method, on main body, allow body reach design standard required article combination;
(2) engraving: adhesive has been carved, cleaned up;
(3) gluing, with above-mentioned mixed transparent resin to describing repeatedly on the goods, to the standard that adheres to specification;
(4) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(5) drying: dried in the shade 30 minutes~1 hour;
(6) drying: with being sprayed on the duplicate from spraying paint, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;

Claims (9)

1, the process for making of ornaments or artificial main stone relief flower pot, its particular-trade is to carry out according to the following steps:
1) simulation:
(1) system wooden mold: timber is sawed, cuts, carves, bondd, the model that joggle becomes to adhere to specification;
(2) system plaster cast: gypsum is added 801 glue, mix well, water and be filled in, after solidifying it is engraved as the model that adheres to specification than in big 0.5~10 centimeter sylphon of model by the mixing of 100: 40~70 ratio;
(3) system mud model: the model that foundry loam or rubber cement kneading model are become to adhere to specification;
(4) engraving: work with great care according to layout;
(5) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(6) bonding: add talcum powder with 502 glue and add saw wood ash=100: 10~30: 10~30;
(7) play putty: add thinner with transparent resin and add curing agent=100: 10~30: 10~30;
(8) polishing: with the sand polishing, from thick number to thin number, to the light cleaning;
(9) go up cured: the floor is cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the model, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
2) system plane soft or hard mould:
(1) system sylphon: vary in size according to model, make the sylphon of different size;
(2) system soft mold: silicon rubber is added curing agent, mix well in 100: 5~20 ratio mixing, brush was being gone up on that cured half model;
(3) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(4) system hard mold: resin is added ketone slurry add and buy liquid and add talcum powder, ratio mixing in 100: 10~30: 10~30: 10~30 is mixed well, brush do not water gypsum mold half soft mold on, spread two layers of fine glass fibre cloth, again above-mentioned hybrid resin is brushed at fine glass fibre cloth, layer overlay thick glass fibre cloth waters above-mentioned hybrid resin and is filled on the thick glass fibre cloth till flood over half 0,5~10 centimeters of thick glass fibre cloth;
(5) drying: dried in the shade 10~30 minutes;
(6) go up cured: analyse ground cured or mould is cured or the spray of table leather board is cured, brush or be sprayed on the soft or hard mould inner wall, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
3) system plane soft mold:
(1) system box: vary in size according to model, make different size, than model big 0.5 centimeter~10 centimeters sylphon;
(2) fixed model: model is placed on the tabula rasa, model bottom packing paper plate or fiber board or plank or laminate, thickness determines what according to goods, goods fill up slab more, and goods fill up rich plate less, after fixing with 502 glue, again the sylphon of making is enclosed within on the model, fixes with 502 glue;
(3) system soft mold: silicon rubber is added curing agent, mix by 100: 5~20 ratio and mix well, water sylphon, till flooding 0.5~10 centimeter on model;
(4) drying: dried in the shade slow curing 2~24 hours 1~2 hour;
(5) die sinking tool: open box, remove tabula rasa, take out the model of the inside;
(6) go up cured: the floor is cured or mould is cured or it is cured to spray the spray of table leather board, brush or be sprayed on the soft mold, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly.
4) the imitative jade material of system: the transparent resin gel coat is added thinner add curing agent=100: 10~30: 10~30.
5) imitative jade material of system and goods:
(1) mould: soft mold is put in the hard mold;
(2) goods: the transparent resin gel coat is added thinner add curing agent, ratio mixing in 100: 10~30: 10~30 is mixed well, water with vessel and to be filled in soft mold or soft or hard mould or hard mold or the gypsum mold, buckle the pressing mold tool, with the limit that a plurality of clips are clamped mould, above-mentioned hybrid resin can't be leached;
(3) drying: dry in the shade to just solidifying;
(4) die sinking tool: open mould, take out early-products;
(5) engraving: early-products is engraved as the goods that adhere to specification;
(6) cool off: goods are placed in the cold water soaked 30 minutes~1 hour;
(7) polishing: the corase grind machine, finish grind by hand, to the light cleaning;
(8) gluing: with above-mentioned mixed transparent resin goods are described repeatedly, till satisfied;
(9) drying: dried in the shade 10~30 minutes;
(1) japanning: with blowing varnish goods are sprayed repeatedly, dried in the shade 15~20 minutes, this step needs 2~3 times repeatedly.
Combination shaping 1:
(1) main body is shaped: by perforating bonding, joggle, grafting method, on main body, allow body reach design standard required article combination;
(2) engraving: adhesive has been carved, cleaned up;
(3) gluing adds thinner with transparent resin and adds curing agent and mix and to mix well, and describes repeatedly on goods, to the effect that adheres to specification;
(4) polishing: carry out with fine sandpaper, from thick number to thin number, to the light cleaning;
(5) drying: dried in the shade 30 minutes~1 hour;
(6) drying: with being sprayed on the duplicate from spraying paint, dried in the shade 15~20 minutes, this step need be carried out 2~3 times repeatedly;
2, model: the preparation method of ornaments according to claim 1 or artificial jade relief flower pot is characterized in that described cast material is that wood, 801 glue add the shape that land plaster=100: 40~70 or foundry loam, rubber sculpture become designing requirement.
3, main body bonding: the preparation method of ornaments according to claim 1 or artificial jade relief flower pot is characterized in that described binding material is that 302 glue or 502 glue add talcum powder and add saw wood ash=100: 10~30: 10~30.
4, moulding: the method for manufacturing technology of ornaments according to claim 1 or artificial jade relief flower pot is characterized in that described Modeling Material is reinforcing bar or steel pipe or iron wire or iron pipe or iron nail or fastener or copper wire or copper pipe.
5, putty: ornaments according to claim 1 or artificial jade relief flower pot process for making, it is characterized in that described putty material is that transparent resin adds thinner and adds curing agent and add talcum powder and add required color=100: 10~30: 10~30: 10~30: 10~30 or atom ash and add curing agent and add required color=100: 10~30: 10~30.
6, soft mold: the process for making of ornaments according to claim 1 or artificial jade relief flower pot is characterized in that described soft model material is that silicon rubber adds curing agent=100: 5~20.
7, hard mold and hollow mould: the process for making of ornaments according to claim 1 or artificial jade relief flower pot, it is characterized in that described hard mold and hollow mould material are that resin adds ketone slurry and adds and buy liquid and add talcum powder=100: 10~30: 10~30: 10~30 and add two layers of fine glass fibre cloth, one deck thick glass fibre cloth.
8, imitative quartzy: the process for making of ornaments according to claim 1 or artificial jade relief flower pot is characterized in that described jade material is that the transparent resin gel coat adds thinner and adds curing agent=100: 10~30: 10~30: 10~30.
9, go up coloring agent: the process for making of the floating pierced carving basin of ornaments according to claim 1 or artificial jade is characterized in that described coloring agent material is that the transparent resin gel coat adds thinner and adds curing agent.
CN 200410070444 2004-08-04 2004-08-04 Process for producing ornaments or artificial jade relief flower pot Pending CN1586123A (en)