CN108942420A - A kind of inner and outer coffin wood surface processing method - Google Patents

A kind of inner and outer coffin wood surface processing method Download PDF

Info

Publication number
CN108942420A
CN108942420A CN201810903049.6A CN201810903049A CN108942420A CN 108942420 A CN108942420 A CN 108942420A CN 201810903049 A CN201810903049 A CN 201810903049A CN 108942420 A CN108942420 A CN 108942420A
Authority
CN
China
Prior art keywords
timber
wood surface
bleaching
air
outer coffin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201810903049.6A
Other languages
Chinese (zh)
Inventor
孟影
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Anhui Batai Arts And Crafts Co Ltd
Original Assignee
Anhui Batai Arts And Crafts Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Anhui Batai Arts And Crafts Co Ltd filed Critical Anhui Batai Arts And Crafts Co Ltd
Priority to CN201810903049.6A priority Critical patent/CN108942420A/en
Publication of CN108942420A publication Critical patent/CN108942420A/en
Pending legal-status Critical Current

Abstract

The present invention discloses a kind of inner and outer coffin wood surface processing method, and the process is the following steps are included: improve defect, anti-corrosion is impregnated, dry polishing, bleaches discoloration, dyeing processing, japanning and chilling treatment.The present invention has carried out improved treatment to timber, is improved first to the defect of wood surface, keeps its surface smooth as much as possible, after anti-corrosion is impregnated, so that timber is not easy to be corroded;Dry polishing step eliminates the impurity and loose particulate material of wood surface, promotes its surface flatness, and the bleaching then carried out and dyeing are handled, and bleaching effect is good, and the surface after bleaching will not change colour for many years, so that the color of wood surface is consistent, it is more beautiful.Last chilling treatment, no longer loose between timber and timber, wood internal structure is more stable.After various step process, the conjugation of finishing coat and timber increases the present invention, not easily to fall off, enhances aesthetics, also improves the service life of timber.

Description

A kind of inner and outer coffin wood surface processing method
Technical field
The present invention relates to inner and outer coffin timber field, a kind of particularly inner and outer coffin wood surface processing method.
Background technique
Timber is the plant for capableing of secondary growth, such as tree and shrubs, is formed by lignified tissue.These plants are first After growth, the vascular cambium in rhizome comes into play, and develops bast outward, inwardly develops timber.
It when timber is used for inner and outer coffin, generally requires to carry out it spray painting processing, needs to pass through natural timber before spray painting It can come into operation after surface-treated, in the prior art, the performance and processing mode of timber own face are gradually by people Ignore, if the surface treatment of timber cannot improve, that will greatly affect the time that spray painting is attached on timber, also can Shorten the service life of timber itself.
Summary of the invention
The purpose of the present invention is to provide a kind of inner and outer coffin wood surface processing methods.
The purpose of the present invention can be achieved through the following technical solutions:
A kind of inner and outer coffin wood surface processing method, the process the following steps are included:
One, improve defect
Pick out the intermediate timber containing large fracture, small holes caused by worms, using with the consistent wooden unit of the same race of wood internal ridge orientation Quick-drying paint is smeared in filling at sections of timber;The resin oozed out uses acid solution or solvent rub, and small crack is filled out with putty It is flat;It is polished flat after quick-drying paint and putty are dry using coarse sandpaper, it is used together with normal lossless plank.
Two, anti-corrosion is impregnated
The more smooth inner and outer coffin timber in surface is selected, the dust and sundries of inner and outer coffin wood surface are removed with air gun, it will be wooden Material, which is put into the pond added with antiseptic solution, to be impregnated 3-5 hours, and the volume ratio of solute and solvent is 1:20, and when immersion makes wood Material is in liquid level always and heating device is arranged in soak with lower portion, while surfactant is added in soak, to It impregnates and completes, take out timber, drain naturally.
Three, dry polishing
Timber is placed in hurricane drier and carries out air-dried, air-drying utensil used is air blower, to timber in air drying process Each orientation air-dries comprehensively up and down, after air-drying to water content less than 15%, is polished with coarse sandpaper wood surface, polishing The powder particle object that wood surface generates is cleaned out using air gun after the completion.
Four, discoloration is bleached
The inner and outer coffin timber of step 3 is laid flat on the table, is floated in the deeper local surfaces of color using bleaching agent White processing, solution is coated on wood surface, stands 20-30 minutes, after the full bleaching of surface, then will with clean wet rag It wipes clean on surface;When bleaching not thorough enough, a small clean cotton gauze of group is immersed in bleaching liquid, is pressed in after taking-up and needs to float Then scrub water wood surface is used until removing cotton gauze after full bleaching in white position, bleaching is completed at this time.
Five, dyeing is handled
Timber of the step 4 after bleached is stood, is dried, configures dyestuff, after mixing, manual brushing applies dyestuff It is put on timber, during which goes through that whether there is or not recess, it is ensured that wood surface is smooth in dyeing course, after standing 2-3 hours Complete dyeing.
Six, japanning
Timber after step 5 is dyed is polished flat using fine sandpaper, then that its removing surface is clean, uses spray Finishing coat is equably sprayed on wood surface by paint rifle, and when spray painting guarantees that finishing coat is smooth, guarantee finishing coat with a thickness of 25-35 μm.
Seven, chilling treatment
Plank taking-up of the step 6 after processed is placed in refrigerating chamber and carries out chilling treatment, the temperature of chilling treatment is 0-2 DEG C, the relative humidity of chilling treatment is 60-70%, and cold preservation time is 5-7 hours, and timber takes out to stand after refrigerating and dry in the air It is dry, the timber of finished product can be obtained.
Further, the coarse sandpaper mesh number is 200 mesh, and fine sandpaper mesh number is 400 mesh.
Further, the wind speed of the air blower blowout is 10m/s, and wind-warm syndrome is 55-65 DEG C, and air-dry time is 2-3 hours.
Further, the bleaching agent selects the mixed liquor of the hydrogen peroxide of 35% concentration and the ammonium hydroxide of 25% concentration, wherein Volume ratio is hydrogen peroxide: water: ammonium hydroxide=1: 1: 0.3.
Further, the dye volume ratio is alcoholic solution dyestuff: alcohol: french polish=8:65:25.
Beneficial effects of the present invention:
The present invention has carried out improved treatment to timber, is improved first to the defect of wood surface, keeps its surface most It is possibly smooth, after anti-corrosion is impregnated, so that timber is not easy to be corroded;Dry polishing step eliminate wood surface impurity and Loose particulate material promotes its surface flatness, and the bleaching then carried out and dyeing are handled, and bleaching effect is good, the surface after bleaching It will not change colour for many years, so that the color of wood surface is consistent, it is more beautiful.Last chilling treatment, between timber and timber not Loose again, wood internal structure is more stable.After various step process, the conjugation of finishing coat and timber increases the present invention, It is not easily to fall off, aesthetics is enhanced, the service life of timber is also improved.
Detailed description of the invention
The present invention will be further described below with reference to the drawings.
Fig. 1 is present invention process method flow schematic diagram.
Specific embodiment
Following will be combined with the drawings in the embodiments of the present invention, and technical solution in the embodiment of the present invention carries out clear, complete Site preparation description, it is clear that described embodiments are only a part of the embodiments of the present invention, instead of all the embodiments.It is based on Embodiment in the present invention, it is obtained by those of ordinary skill in the art without making creative efforts all other Embodiment shall fall within the protection scope of the present invention.
In the description of the present invention, it is to be understood that, term " aperture ", "upper", "lower", " thickness ", "top", " in ", Indicating positions or the positional relationship such as " length ", "inner", " surrounding ", are merely for convenience of description of the present invention and simplification of the description, without It is that the component of indication or suggestion meaning or element must have a particular orientation, is constructed and operated in a specific orientation, therefore not It can be interpreted as limitation of the present invention.
A kind of inner and outer coffin wood surface processing method, as shown in Figure 1, the process the following steps are included:
One, improve defect
Pick out the intermediate timber containing large fracture, small holes caused by worms, using with the consistent wooden unit of the same race of wood internal ridge orientation Quick-drying paint, such as shellac varnish, zapon confining surface are smeared in filling at sections of timber, and resin is oozed out after preventing;It has seeped Resin out uses acid solution or solvent rub, and small crack is filled and led up with putty.It is thick using 200 mesh after quick-drying paint and putty are dry Sand paper polishes flat, it is used together with normal lossless plank.
Two, anti-corrosion is impregnated
The more smooth inner and outer coffin timber in surface is selected, the dust and sundries of inner and outer coffin wood surface are removed with air gun, it will be wooden Material, which is put into the pond added with antiseptic solution, to be impregnated 3-5 hours, and the volume ratio of solute and solvent is 1:20, and when immersion makes wood Material is in liquid level always and heating device is arranged in soak with lower portion, while surfactant is added in soak, adds Thermal and surfactant can improve the permeability of timber, complete wait impregnate, and take out timber, drain naturally, at this time timber There are anti-corrosive properties, be not easy to be corroded.
Three, dry polishing
Timber is placed in hurricane drier and carries out air-dried, air-drying utensil used is air blower, and the wind speed of air blower blowout is 10m/s, wind-warm syndrome are 55-65 DEG C, and air-dry time is 2-3 hours, and to timber, each orientation is comprehensive up and down in air drying process It air-dries, after air-drying to water content less than 15%, is polished with 200 mesh coarse sandpapers wood surface, air gun is used after the completion of polishing The powder particle object that wood surface generates is cleaned out.
Four, discoloration is bleached
The inner and outer coffin timber of step 3 is laid flat on the table, is floated in the deeper local surfaces of color using bleaching agent White processing, bleaching agent select the mixed liquor of the hydrogen peroxide of 35% concentration and the ammonium hydroxide of 25% concentration, and wherein volume ratio is hydrogen peroxide: Water: ammonium hydroxide=1: 1: 0.3, solution is coated on wood surface, stand 20-30 minute, after the full bleaching of surface, then with clean Wet rag surface is wiped clean;When bleaching not thorough enough, a small clean cotton gauze of group is immersed in bleaching liquid, after taking-up It is pressed in the position for needing to bleach, until removing cotton gauze after full bleaching, scrub water wood surface is then used, has bleached at this time At.Such method is fine for the bleaching effect of timber, and the surface after bleaching will not change colour for many years.
Five, dyeing is handled
Timber of the step 4 after bleached is stood, is dried.Dyestuff is configured, weighing volume ratio is alcoholic solution dyestuff: alcohol: French polish=8:65:25 dyestuff, after mixing, dyestuff is applied on timber by manual brushing, has during which been gone through Without recess, it is ensured that wood surface is smooth in dyeing course, and dyeing can be completed after standing 2-3 hours.Such colouring method alcohol It is volatile, but nonwetting timber, fluffy phenomenon is eliminated, and dye in bright gay color, the obtained grain of wood is graceful, Color is uniform.
Six, japanning
Timber after step 5 is dyed is polished flat using the fine sandpaper that mesh number is 400 mesh, then that its surface is clear Reason is clean, and finishing coat is equably sprayed on wood surface using spray gun for paint, and when spray painting guarantees that finishing coat is smooth, guarantee finishing coat with a thickness of 25-35μm。
Seven, chilling treatment
Plank taking-up of the step 6 after processed is placed in refrigerating chamber and carries out chilling treatment, the temperature of chilling treatment is 0-2 DEG C, the relative humidity of chilling treatment is 60-70%, and cold preservation time is 5-7 hours, and timber is after chilling treatment, in timber Portion's structure is more stable.Timber, which takes out to stand after refrigerating, to be dried, and the timber of finished product can be obtained.
In the description of this specification, the description of reference term " one embodiment ", " example ", " specific example " etc. means Particular features, structures, materials, or characteristics described in conjunction with this embodiment or example are contained at least one implementation of the invention In example or example.In the present specification, schematic expression of the above terms may not refer to the same embodiment or example. Moreover, particular features, structures, materials, or characteristics described can be in any one or more of the embodiments or examples to close Suitable mode combines.
The basic principles, main features and advantages of the present invention have been shown and described above.The technology of the industry Personnel are it should be appreciated that the present invention is not limited to the above embodiments, and the above embodiments and description only describe this The principle of invention, without departing from the spirit and scope of the present invention, various changes and improvements may be made to the invention, these changes Change and improvement all fall within the protetion scope of the claimed invention.

Claims (5)

1. a kind of inner and outer coffin wood surface processing method, which is characterized in that the process the following steps are included:
One, improve defect
The intermediate timber containing large fracture, small holes caused by worms is picked out, is clogged using with the consistent wooden unit of the same race of wood internal ridge orientation, Quick-drying paint is smeared at sections of timber;The resin oozed out uses acid solution or solvent rub, and small crack is filled and led up with putty;To fast It is polished flat after dried lacquer and putty are dry using coarse sandpaper, it is used together with normal lossless plank;
Two, anti-corrosion is impregnated
The more smooth inner and outer coffin timber in surface is selected, the dust and sundries of inner and outer coffin wood surface are removed with air gun, timber is put Enter in the pond added with antiseptic solution and impregnate 3-5 hours, the volume ratio of solute and solvent is 1:20, and when immersion makes timber begin Heating device is arranged in soak with lower portion in liquid level eventually, while adding surfactant in soak, wait impregnate It completes, takes out timber, drain naturally;
Three, dry polishing
Timber is placed in hurricane drier and carries out air-dried, air-drying utensil used is air blower, in air drying process to timber above and below The each orientation in left and right air-dries comprehensively, after air-drying to water content less than 15%, is polished with coarse sandpaper wood surface, polishing is completed The powder particle object that wood surface generates is cleaned out using air gun afterwards;
Four, discoloration is bleached
The inner and outer coffin timber of step 3 is laid flat on the table, is carried out at bleaching in the deeper local surfaces of color using bleaching agent Reason, solution is coated on wood surface, stands 20-30 minutes, after the full bleaching of surface, then with clean wet rag by surface It wipes clean;When bleaching not thorough enough, a small clean cotton gauze of group is immersed in bleaching liquid, is pressed in what needs were bleached after taking-up Then scrub water wood surface is used until removing cotton gauze after full bleaching in position, bleaching is completed at this time;
Five, dyeing is handled
Timber of the step 4 after bleached is stood, is dried, configures dyestuff, after mixing, dyestuff is applied to by manual brushing On timber, during which go through that whether there is or not recess, it is ensured that wood surface is smooth in dyeing course, can be completed after standing 2-3 hours Dyeing;
Six, japanning
Timber after step 5 is dyed is polished flat using fine sandpaper, then that its removing surface is clean, uses spray gun for paint Finishing coat is equably sprayed on wood surface, when spray painting, guarantees that finishing coat is smooth, guarantee finishing coat with a thickness of 25-35 μm;
Seven, chilling treatment
Plank taking-up of the step 6 after processed is placed in refrigerating chamber and carries out chilling treatment, the temperature of chilling treatment is 0-2 DEG C, the relative humidity of chilling treatment is 60-70%, and cold preservation time is 5-7 hours, and timber, which takes out to stand after refrigerating, to be dried, The timber of finished product can be obtained.
2. a kind of inner and outer coffin wood surface processing method according to claim 1, which is characterized in that the coarse sandpaper mesh number is 200 mesh, fine sandpaper mesh number are 400 mesh.
3. a kind of inner and outer coffin wood surface processing method according to claim 1, which is characterized in that the air blower blowout Wind speed is 10m/s, and wind-warm syndrome is 55-65 DEG C, and air-dry time is 2-3 hours.
4. a kind of inner and outer coffin wood surface processing method according to claim 1, which is characterized in that the bleaching agent is selected The mixed liquor of the hydrogen peroxide of 35% concentration and the ammonium hydroxide of 25% concentration, wherein volume ratio is hydrogen peroxide: water: ammonium hydroxide=1: 1: 0.3.
5. a kind of inner and outer coffin wood surface processing method according to claim 1, which is characterized in that the dye volume ratio is Alcoholic solution dyestuff: alcohol: french polish=8:65:25.
CN201810903049.6A 2018-08-09 2018-08-09 A kind of inner and outer coffin wood surface processing method Pending CN108942420A (en)