CN107059487A - The preparation method of 30 grams of facing papers - Google Patents
The preparation method of 30 grams of facing papers Download PDFInfo
- Publication number
- CN107059487A CN107059487A CN201710175611.3A CN201710175611A CN107059487A CN 107059487 A CN107059487 A CN 107059487A CN 201710175611 A CN201710175611 A CN 201710175611A CN 107059487 A CN107059487 A CN 107059487A
- Authority
- CN
- China
- Prior art keywords
- grams
- paper
- printing
- casein
- preparation
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of preparation method of 30 grams of facing papers, comprise the following steps:Step one, prepare, casein milk storage is prepared by raw material of casein, water, setting agent and alcohol standby;Obtained casein milk in step one is injected into coating machine by step 2, coating, and 30 grams of body paper are led through to coating machine, sizing paper is made in the backsize casein milk of 30 grams of body paper;Step 3, printing leads sizing paper through to printing machine, carrying out printing in sizing recto and printing paper being made, and sizing paper is placed on belt conveyor in printing process to carry out delivery;Step 4, drying leads printing paper through to drying baker, drying and 30 grams of facing papers being made.The present invention can produce 30 grams of facing papers, be made by whole wood pulp and filler, aqueous, environmental protective, green organic, be conducive to health, and the cost of product is low, and consume energy low, good permeability, and performance is good, and intensity is high.
Description
Technical field
The present invention relates to a kind of preparation method of facing paper, more particularly to a kind of preparation method of 30 grams of facing papers.
Background technology
At present, China's traditional decoration paper is 70~120 grams of facing papers, and China consumes 670,000 tons of traditional decoration paper every year, often
Ton traditional decoration paper takes around 380 kilograms of import pulps, and traditional decoration paper quantity per ton is about 4500, traditional high-side dress
The price for adoring paper is 1.5 ten thousand yuan/ton, and cost is higher, expensive.Because the body paper coefficient of expansion is big, water imbibition is big, immersing glue process
In be easily broken off, crumple, the limit of existing production technology is 70 grams of facing papers of production.70~80 grams of traditional decoration paper gas permeabilities compared with
It could be permeated completely within 35~45 seconds under difference, 100ml water vacuum conditions.The number of 70~80 grams of traditional decoration paper impregnated melamine glue
Measure and put down for 140~170g/, spread is big.The drying temperature of 70~80 grams of traditional decoration paper is 160~180 DEG C, and drying rate is
100~150 meters/min, drying efficiency is poor.At present, the technology of 30 grams of facing papers, existing 30 grams are not produced using whole wood pulp
Facing paper, such as polywood paper are using bamboo prize, wood pulp and wet strengthening resin, due to containing inorganic pigment and benzene dilution, being unfavorable for environment
Protection, it is harmful.
The content of the invention
The present invention provides a kind of preparation method of 30 grams of facing papers, 30 grams of facing papers can be produced, by whole wood pulp and filler
It is made, aqueous, environmental protective, green organic is conducive to health, and the cost of product is low, consume energy low, good permeability, performance is good, by force
Degree is high.
In order to solve the above technical problems, the technical scheme is that:A kind of preparation method of 30 grams of facing papers, including with
Lower step:
Step one, prepare, casein milk storage is prepared by raw material of casein, water, setting agent and alcohol standby;
Obtained casein milk in step one is injected into coating machine by step 2, coating, and 30 grams of body paper are led through to painting
Cloth machine, sizing paper is made in the backsize casein milk of 30 grams of body paper;
Step 3, printing leads sizing paper through to printing machine, carrying out printing in sizing recto and printing paper being made, and
Sizing paper is placed on belt conveyor in printing process and carries out delivery;
Step 4, drying leads printing paper through to drying baker, drying and 30 grams of facing papers being made.
As preferred technical scheme, step one process for preparation is specially:Injected according to mass fraction to reactor
10~20 parts of water and 7~12 parts of alcohol, then 65~75 parts of casein stirring and dissolving is put into, add 3~7 parts of sizing
Agent, stir obtained casein milk.
As the improvement to above-mentioned technical proposal, in the step 2 coating process, casein milk is injected into coating
Before machine, first casein milk is stirred, viscous consistency is adjusted.
As the further improvement to above-mentioned technical proposal, in the step 2 coating process, coating casein milk tool
Body is that, in 3~5 grams of casein milks of backsize of every square of 30 grams of body paper, 30 grams of body paper are with 150~200 meters/min speed
Degree passes through coating machine, and the coating temperature of coating machine is 90~120 DEG C.
As the further improvement to above-mentioned technical proposal, the step 4 drying course is specially six sections of temperature bakings
Dry, drying temperature is followed successively by 120 DEG C, 135 DEG C, 145 DEG C, 160 DEG C, 145 DEG C and 120 DEG C.
As the further improvement to above-mentioned technical proposal, in step 2, obtained sizing paper is led through to rewinding machine
Rewinding is into paper bowl.
As especially further improving to above-mentioned technical proposal, step 5 overlays, 30 grams of facing papers of step 4 is led
Through to hot press, 150~170 DEG C of temperature is overlayed 15~25 seconds;
Step 6, plate is cut out, the sheet material that cutting step five has been overlayed.
By adopting the above-described technical solution, shaped by Paper Coating, 30 grams of paper that modified technique process for producing goes out, by
Whole wood pulp and filler are made, aqueous, environmental protective, green organic, are conducive to health, and chromatography is accurate, resists and crumples, and each performance
Better than existing 70~80g like products, 30 grams of facing paper quantity per ton are about 9500 or so, and quantity is more, and cost is low, are needed
The import pulp wanted can decline 55%, reduce deforestation.30 grams of facing paper gas permeabilities are improved, and 100ml water vacuum 13~
Infiltration completely in 20 seconds.In 30 grams of facing paper production processes, it can be led with the condition of 120~160 DEG C, 150~200 meters/min through drying
Dry case, drying temperature is low, and drying rate is very fast.The present invention can produce 30 grams of facing papers, be made by whole wood pulp and filler, aqueous
Environmental protection, green organic is conducive to health, and the cost of product is low, and consume energy low, good permeability, and performance is good, and intensity is high.
Brief description of the drawings
The following drawings is only intended to, in doing schematic illustration and explanation to the present invention, not delimit the scope of the invention.Wherein:
Fig. 1 is the schematic flow sheet of the embodiment of the present invention.
Embodiment
With reference to embodiment and accompanying drawing, the present invention is expanded on further.In the following detailed description, only explanation is passed through
Mode describes some one exemplary embodiments of the present invention.Undoubtedly, one of ordinary skill in the art will recognize,
In the case of without departing from the spirit and scope of the present invention, described embodiment can be repaiied with a variety of modes
Just.Therefore, describe inherently illustrative, be not intended to limit the scope of the claims.
As long as in addition, technical characteristic involved in each embodiment of invention described below non-structure each other
It can be just mutually combined into conflict.
As shown in figure 1, a kind of preparation method of 30 grams of facing papers, comprises the following steps:
Step one, prepare, casein milk storage is prepared by raw material of casein, water, setting agent and alcohol standby;
Obtained casein milk in step one is injected into coating machine by step 2, coating, and 30 grams of body paper are led through to painting
Cloth machine, sizing paper is made in the backsize casein milk of 30 grams of body paper;
Step 3, printing leads sizing paper through to printing machine, carrying out printing in sizing recto and printing paper being made, and
Sizing paper is placed on belt conveyor in printing process and carries out delivery, printing process uses conveyer belt delivery, effectively prevents paper
Fracture;
Step 4, drying leads printing paper through to drying baker, drying and 30 grams of facing papers being made.
Shaped by Paper Coating, 30 grams of paper that modified technique process for producing goes out, be made by whole wood pulp and filler, aqueous ring
Protect, green organic, be conducive to health, chromatography is accurate, resists and crumples, and each performance is better than existing 70~80g like products,
30 grams of facing paper quantity per ton are about 9500 or so, and quantity is more, cost it is low, it is necessary to import pulp can decline
55%, reduce deforestation.30 grams of facing paper gas permeabilities are improved, the infiltration completely in 13~20 seconds of 100ml water vacuum.30 grams of decorations
In paper production process, drying case can be led with the condition of 120~160 DEG C, 150~200 meters/min, drying temperature is low, dried
Speed.
Step one process for preparation is specially:According to mass fraction to reactor inject 10~20 parts water and 7~12 parts
Alcohol, then 65~75 parts of casein stirring and dissolving is put into, 3~7 parts of setting agent is added, stir obtained casein breast
Liquid.The casein milk that above-mentioned steps are produced can preferably increase the intensity of 30 grams of body paper, be conducive to printing-ink of shaping,
So that chromatography is accurate, resists and crumples.
In step 2 coating process, casein milk is injected into before coating machine, first casein milk stirred, is adjusted
Whole viscous consistency, above-mentioned steps are conducive to even spread casein milk.
In step 2 coating process, coating casein milk is specifically, in the backsize 3~5 of every square of 30 grams of body paper
Gram casein milk, 30 grams of body paper pass through coating machine with 150~200 meters/min speed, the coating temperature of coating machine for 90~
120 DEG C, above-mentioned steps are able to ensure that the coating of casein milk.
Step 4 drying course is specially the drying of six sections of temperature, drying temperature be followed successively by 120 DEG C, 135 DEG C, 145 DEG C, 160
DEG C, 145 DEG C and 120 DEG C.Printing paper is led through to drying baker, drying temperature is low, speed with 150~200 meters/min speed,
The energy of consumption is low.
In step 2, obtained sizing paper is led through to rewinding machine rewinding into paper bowl, above-mentioned steps are easy to detection sizing paper
Quality.
Step 5, is overlayed, and 30 grams of facing papers of step 4 is led through to hot press, 150~170 DEG C of temperature, overlay 15~
25 seconds;Step 6, plate is cut out, the sheet material that cutting step five has been overlayed;Above-mentioned steps are easy to the direct application of 30 grams of facing papers.
The present embodiment can produce 30 grams of facing papers, be made by whole wood pulp and filler, aqueous, environmental protective, green organic, favorably
In health, the cost of product is low, and consume energy low, good permeability, and performance is good, and intensity is high.
General principle, principal character and the advantages of the present invention of the present invention has been shown and described above.The technology of the industry
Personnel are it should be appreciated that the present invention is not limited to the above embodiments, and the simply explanation described in above-described embodiment and specification is originally
The principle of invention, without departing from the spirit and scope of the present invention, various changes and modifications of the present invention are possible, these changes
Change and improvement all fall within the protetion scope of the claimed invention.The claimed scope of the invention by appended claims and its
Equivalent thereof.
Claims (7)
1. a kind of preparation method of 30 grams of facing papers, it is characterised in that comprise the following steps:
Step one, prepare, casein milk storage is prepared by raw material of casein, water, setting agent and alcohol standby;
Obtained casein milk in step one is injected into coating machine by step 2, coating, and 30 grams of body paper are led through to coating
Machine, sizing paper is made in the backsize casein milk of 30 grams of body paper;
Step 3, printing leads sizing paper through to printing machine, carrying out printing in sizing recto and printing paper, and printing being made
During sizing paper is placed on belt conveyor and carries out delivery;
Step 4, drying leads printing paper through to drying baker, drying and 30 grams of facing papers being made.
2. the preparation method of 30 grams of facing papers as claimed in claim 1, it is characterised in that step one process for preparation is specific
For:10~20 parts of water and 7~12 parts of alcohol are injected to reactor according to mass fraction, then puts into 65~75 parts of casein
Stirring and dissolving, adds 3~7 parts of setting agent, stir obtained casein milk.
3. the preparation method of 30 grams of facing papers as claimed in claim 1, it is characterised in that in the step 2 coating process,
Casein milk is injected into before coating machine, first casein milk stirred, viscous consistency is adjusted.
4. the preparation method of 30 grams of facing papers as claimed in claim 1, it is characterised in that in the step 2 coating process,
Casein milk is coated with specifically, in 3~5 grams of casein milks of backsize of every square of 30 grams of body paper, 30 grams of body paper are with 150
~200 meters/min speed passes through coating machine, and the coating temperature of coating machine is 90~120 DEG C.
5. the preparation method of 30 grams of facing papers as claimed in claim 1, it is characterised in that the step 4 drying course is specific
For six sections of temperature drying, drying temperature is followed successively by 120 DEG C, 135 DEG C, 145 DEG C, 160 DEG C, 145 DEG C and 120 DEG C.
6. the preparation method of 30 grams of facing papers as claimed in claim 1, it is characterised in that in step 2, by obtained sizing
Paper is led through to rewinding machine rewinding into paper bowl.
7. the preparation method of 30 grams of facing papers as described in any one of claim 1 to 6, it is characterised in that also include:Step
Five, overlay, 30 grams of facing papers of step 4 are led through to hot press, 150~170 DEG C of temperature is overlayed 15~25 seconds;
Step 6, plate is cut out, the sheet material that cutting step five has been overlayed.