CN106427370A - Process for lacquer painting graining through prefabricated ice blocks - Google Patents
Process for lacquer painting graining through prefabricated ice blocks Download PDFInfo
- Publication number
- CN106427370A CN106427370A CN201610836585.XA CN201610836585A CN106427370A CN 106427370 A CN106427370 A CN 106427370A CN 201610836585 A CN201610836585 A CN 201610836585A CN 106427370 A CN106427370 A CN 106427370A
- Authority
- CN
- China
- Prior art keywords
- paint
- lacquer
- graining
- lacquer painting
- producing ice
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
The invention discloses a process for lacquer painting graining through prefabricated ice blocks. Through ice block prefabrication, lacquer base preparation, lacquer preparation, undercoat smearing, prefabricated ice block laying, extrusion forming, lacquer coating, grinding, pushing polishing and wiping cleaning steps, the process for lacquer painting graining through the prefabricated ice blocks is completed. Through the process, the final effect controllability of lacquer painting graining can be improved effectively, adhesion of lacquer and a graining tool or a medium during graining is reduced, the precision of a pattern is ensured, grain uniformity of a plurality of pictures is ensured, the requirement of mass production is met, the links for tool or medium cleaning are reduced, energy conservation and environment protection are achieved, and the cost is low. On the premise that the picture effect is not influenced, the picture making efficiency is improved, the picture forming time is shortened, the picture making process is simplified, the process is convenient, and industrial production is easy.
Description
Technical field
The invention belongs to a kind of lacquer painting graining technique is and in particular to a kind of work carrying out lacquer painting graining using pre- producing ice cakes
Skill.
Background technology
At present, the change painting of paint skill field is divided into following several ways:Instrument graining, vehicle graining, powder material graining, slow release
Agent graining etc., common are in instrument graining:With ball wimple stricture of vagina, with hair brush graining, with Cornu Bovis seu Bubali scraper graining etc.;Medium
Having of thing graining is medium graining, is medium graining, is pressed paint graining etc. with silk screen with Semen sojae atricolor with Folium Pini or Cacumen Cupressi;Powder material rises
The having with tobacco shred graining, broken coat of paint graining etc. of stricture of vagina, but, above graining method is required for producer by long-term experience accumulation,
Trick cooperation puts in place and just can reach ideal effect.Required precision for texture higher it is ensured that mass product texture one
Cause property, reach volume production requirement lacquer painting texture mould for, traditional technique seems awkward sometimes, and this is accomplished by change and follows
Rule step the conservative idea of square, develop and use new medium materials and means.
Content of the invention
Present invention aims to the deficiencies in the prior art, now provide a kind of energy-conserving and environment-protective, cost relatively low, in not shadow
On the premise of ringing picture effect, effectively improve picture efficiency processed, that shortens into the picture time carries out lacquer painting graining using pre- producing ice cakes
Technique.
For solving above-mentioned technical problem, the technical solution used in the present invention is:One kind carries out lacquer painting using pre- producing ice cakes and rises
The technique of stricture of vagina, its innovative point is:Through pre- producing ice cakes, preparation paint tire, standby paint, prime, lay pre- producing ice cakes, be squeezed into
Type, coat with lacquer paint, mill show, push away light and wipe clear step, the technique completing to carry out lacquer painting graining using pre- producing ice cakes;Comprise the following steps that:
(1)Pre- producing ice cakes:Water is poured in the mould of plastics carrying out respective texture in advance, putting into refrigerator-freezer, to be cooled to subzero 18 Celsius
Degree, until water freezes completely, standby;
(2)Prepare paint tire:Selected import five-ply board is as base plate, smooth using liquid honing, then passes through latex in base plate
On mount one layer of mull, dismiss unnecessary mull after drying, standby;(3)Standby paint:Take Resina Toxicodendri verniciflui, thin dark grey to be in harmonious proportion uniformly, be obtained
Under-coating varnish, the mixing quality of described Resina Toxicodendri verniciflui and thin dark grey is than for 1:1-2;(4)Prime:By uniform for under-coating varnish brush in paint tire
On, brush 3-5 time;(5)Lay pre- producing ice cakes:The mould of plastics filling ice is placed 1-2 minute at normal temperatures, is allowed to micro- and melts,
Ice cube is carefully taken out from mould of plastics, is put as requested, veined face is flattened on priming paint;(6)Extruding
Molding:Pressing ice cube, is allowed to form corrugation pattern on lacquer painting, removes ice cube, treat that frozen water dries, such as ice cube does not damage, permissible
Scribble in second, third width and reuse in the paint version of priming paint, until on ice cube pattern damaged it is impossible to till use;(7)Coat with lacquer
Paint:Cover upper colored paint on request, repeat to coat with lacquer paint step 2-5 time after dry;(8)Mill is aobvious:Carefully grind aobvious, to its lacquer painting, nature occurs
Texture;(9)Push away light:Take transparent polished lacquer, dipped in Cotton Gossypii and carry out pushing repeatedly on lacquer painting surface;(10)Wipe clear:Use
Absorbent cotton dips in a certain amount of raw vegetable oil of addition, smears uniformly on lacquer painting.
Further, described step(10)In raw vegetable oil smearing thickness be 0.01-0.04mm.
Beneficial effects of the present invention are as follows:The final effect controllability of lacquer painting graining can be effectively improved using the present invention,
Reduce during graining with the adhesion playing rasp tool or medium it is ensured that the precision of grain pattern, it is ensured that multiple picture texture homogeneity, meets and criticizes
Quantify production requirement, reduce the link of cleaning tool or medium, energy-conserving and environment-protective, cost are relatively low, before not affecting picture effect
Put, improve picture efficiency processed, shorten into the picture time, simplify picture making craft, technique convenient it is easy to industrialized production.
Specific embodiment
Hereinafter embodiments of the present invention are illustrated by particular specific embodiment, those skilled in the art can be by this explanation
Content disclosed by book understands other advantages and effect of the present invention easily.
Embodiment 1
A kind of technique being carried out lacquer painting graining using pre- producing ice cakes, through pre- producing ice cakes, preparation paint tire, standby painted, primes, laying
Pre- producing ice cakes, extrusion molding, coat with lacquer paint, mill show, push away light and wipe clear step, complete to carry out the work of lacquer painting graining using pre- producing ice cakes
Skill;Comprise the following steps that:
(1)Pre- producing ice cakes:Water is poured in the mould of plastics carrying out respective texture in advance, putting into refrigerator-freezer, to be cooled to subzero 18 Celsius
Degree, until water freezes completely, standby;
(2)Prepare paint tire:Selected import five-ply board is as base plate, smooth using liquid honing, then passes through latex in base plate
On mount one layer of mull, dismiss unnecessary mull after drying, standby;(3)Standby paint:Take Resina Toxicodendri verniciflui, thin dark grey to be in harmonious proportion uniformly, be obtained
Under-coating varnish, the mixing quality of Resina Toxicodendri verniciflui and thin dark grey is than for 1:1;(4)Prime:By uniform for under-coating varnish brush on paint tire, brushing
3 times;(5)Lay pre- producing ice cakes:The mould of plastics filling ice is placed 1 minute at normal temperatures, is allowed to micro- and melts, by ice cube from moulding
Carefully take out in material mould, put as requested, veined face is flattened on priming paint;(6)Extrusion molding:Pressing
Ice cube, is allowed to form corrugation pattern on lacquer painting, removes ice cube, treat that frozen water dries, such as ice cube does not damage, can second, the
Three width scribble to be reused in the paint version of priming paint, until on ice cube pattern damaged it is impossible to till use;(7)Coat with lacquer paint:On request
Colored paint on cover, repeats to coat with lacquer paint step 2 time after dry;(8)Mill is aobvious:Carefully grind aobvious, to its lacquer painting, natural texture occurs;(9)
Push away light:Take transparent polished lacquer, dipped in Cotton Gossypii and carry out pushing repeatedly on lacquer painting surface;(10)Wipe clear:Dipped in using absorbent cotton and add
Enter a certain amount of raw vegetable oil, lacquer painting is smeared uniformly, the smearing thickness of raw vegetable oil is 0.01mm.
Embodiment 2
A kind of technique being carried out lacquer painting graining using pre- producing ice cakes, through pre- producing ice cakes, preparation paint tire, standby painted, primes, laying
Pre- producing ice cakes, extrusion molding, coat with lacquer paint, mill show, push away light and wipe clear step, complete to carry out the work of lacquer painting graining using pre- producing ice cakes
Skill;Comprise the following steps that:
(1)Pre- producing ice cakes:Water is poured in the mould of plastics carrying out respective texture in advance, putting into refrigerator-freezer, to be cooled to subzero 18 Celsius
Degree, until water freezes completely, standby;
(2)Prepare paint tire:Selected import five-ply board is as base plate, smooth using liquid honing, then passes through latex in base plate
On mount one layer of mull, dismiss unnecessary mull after drying, standby;(3)Standby paint:Take Resina Toxicodendri verniciflui, thin dark grey to be in harmonious proportion uniformly, be obtained
Under-coating varnish, the mixing quality of Resina Toxicodendri verniciflui and thin dark grey is than for 1:2;(4)Prime:By uniform for under-coating varnish brush on paint tire, brushing
5 times;(5)Lay pre- producing ice cakes:The mould of plastics filling ice is placed 2 minutes at normal temperatures, is allowed to micro- and melts, by ice cube from moulding
Carefully take out in material mould, put as requested, veined face is flattened on priming paint;(6)Extrusion molding:Pressing
Ice cube, is allowed to form corrugation pattern on lacquer painting, removes ice cube, treat that frozen water dries, such as ice cube does not damage, can second, the
Three width scribble to be reused in the paint version of priming paint, until on ice cube pattern damaged it is impossible to till use;(7)Coat with lacquer paint:On request
Colored paint on cover, repeats to coat with lacquer paint step 5 time after dry;(8)Mill is aobvious:Carefully grind aobvious, to its lacquer painting, natural texture occurs;(9)
Push away light:Take transparent polished lacquer, dipped in Cotton Gossypii and carry out pushing repeatedly on lacquer painting surface;(10)Wipe clear:Dipped in using absorbent cotton and add
Enter a certain amount of raw vegetable oil, lacquer painting is smeared uniformly, the smearing thickness of raw vegetable oil is 0.04mm.
Embodiment 3
A kind of technique being carried out lacquer painting graining using pre- producing ice cakes, through pre- producing ice cakes, preparation paint tire, standby painted, primes, laying
Pre- producing ice cakes, extrusion molding, coat with lacquer paint, mill show, push away light and wipe clear step, complete to carry out the work of lacquer painting graining using pre- producing ice cakes
Skill;Comprise the following steps that:
(1)Pre- producing ice cakes:Water is poured in the mould of plastics carrying out respective texture in advance, putting into refrigerator-freezer, to be cooled to subzero 18 Celsius
Degree, until water freezes completely, standby;
(2)Prepare paint tire:Selected import five-ply board is as base plate, smooth using liquid honing, then passes through latex in base plate
On mount one layer of mull, dismiss unnecessary mull after drying, standby;(3)Standby paint:Take Resina Toxicodendri verniciflui, thin dark grey to be in harmonious proportion uniformly, be obtained
Under-coating varnish, the mixing quality of Resina Toxicodendri verniciflui and thin dark grey is than for 1:1.5;(4)Prime:By uniform for under-coating varnish brush on paint tire, apply
Brush 4 times;(5)Lay pre- producing ice cakes:The mould of plastics filling ice is placed 1.5 minutes at normal temperatures, is allowed to micro- and melts, by ice cube
Carefully take out from mould of plastics, put as requested, veined face is flattened on priming paint;(6)Extrusion molding:
Pressing ice cube, is allowed to form corrugation pattern on lacquer painting, removes ice cube, treat that frozen water dries, such as ice cube does not damage, can be the
2nd, the 3rd width scribbles and reuses in the paint version of priming paint, until on ice cube pattern damaged it is impossible to till use;(7)Coat with lacquer paint:Press
Require the upper colored paint of cover, repeat to coat with lacquer paint step 4 time after dry;(8)Mill is aobvious:Carefully grind aobvious, to its lacquer painting, natural texture occurs;
(9)Push away light:Take transparent polished lacquer, dipped in Cotton Gossypii and carry out pushing repeatedly on lacquer painting surface;(10)Wipe clear:Dipped in using absorbent cotton
A certain amount of raw vegetable oil of upper addition, smears uniformly on lacquer painting, and the smearing thickness of raw vegetable oil is 0.025mm.
Can effectively improve the final effect controllability of lacquer painting graining using the present invention, reduce during graining with rise rasp tool or
The adhesion of medium is it is ensured that the precision of grain pattern, it is ensured that multiple picture texture homogeneity, meets mass production requirement, reduces cleaning
Instrument or the link of medium, energy-conserving and environment-protective, cost are relatively low, on the premise of not affecting picture effect, improve picture efficiency processed, contracting
The short one-tenth picture time, simplify picture making craft, technique convenient it is easy to industrialized production.
Above-described embodiment is presently preferred embodiments of the present invention, is not the restriction to technical solution of the present invention, as long as
The technical scheme that can realize on the basis of above-described embodiment without creative work, is regarded as falling into patent of the present invention
Rights protection scope in.
Claims (2)
1. a kind of using pre- producing ice cakes carry out lacquer painting graining technique it is characterised in that:Through pre- producing ice cakes, preparation paint tire, standby
Paint, prime, lay pre- producing ice cakes, extrusion molding, coat with lacquer paint, mill show, push away light and wipe clear step, complete to carry out using pre- producing ice cakes
The technique of lacquer painting graining;Comprise the following steps that:
(1)Pre- producing ice cakes:Water is poured in the mould of plastics carrying out respective texture in advance, putting into refrigerator-freezer, to be cooled to subzero 18 Celsius
Degree, until water freezes completely, standby;
(2)Prepare paint tire:Selected import five-ply board is as base plate, smooth using liquid honing, then passes through latex in base plate
On mount one layer of mull, dismiss unnecessary mull after drying, standby;(3)Standby paint:Take Resina Toxicodendri verniciflui, thin dark grey to be in harmonious proportion uniformly, be obtained
Under-coating varnish, the mixing quality of described Resina Toxicodendri verniciflui and thin dark grey is than for 1:1-2;(4)Prime:By uniform for under-coating varnish brush in paint tire
On, brush 3-5 time;(5)Lay pre- producing ice cakes:The mould of plastics filling ice is placed 1-2 minute at normal temperatures, is allowed to micro- and melts,
Ice cube is carefully taken out from mould of plastics, is put as requested, veined face is flattened on priming paint;(6)Extruding
Molding:Pressing ice cube, is allowed to form corrugation pattern on lacquer painting, removes ice cube, treat that frozen water dries, such as ice cube does not damage, permissible
Scribble in second, third width and reuse in the paint version of priming paint, until on ice cube pattern damaged it is impossible to till use;(7)Coat with lacquer
Paint:Cover upper colored paint on request, repeat to coat with lacquer paint step 2-5 time after dry;(8)Mill is aobvious:Carefully grind aobvious, to its lacquer painting, nature occurs
Texture;(9)Push away light:Take transparent polished lacquer, dipped in Cotton Gossypii and carry out pushing repeatedly on lacquer painting surface;(10)Wipe clear:Use
Absorbent cotton dips in a certain amount of raw vegetable oil of addition, smears uniformly on lacquer painting.
2. according to claim 1 a kind of using pre- producing ice cakes carry out lacquer painting graining technique it is characterised in that:Described step
Suddenly(10)In raw vegetable oil smearing thickness be 0.01-0.04mm.