CN106391815A - Device and method for improving uniformity of wall thickness of stamping deep drawing part - Google Patents

Device and method for improving uniformity of wall thickness of stamping deep drawing part Download PDF

Info

Publication number
CN106391815A
CN106391815A CN201610952055.1A CN201610952055A CN106391815A CN 106391815 A CN106391815 A CN 106391815A CN 201610952055 A CN201610952055 A CN 201610952055A CN 106391815 A CN106391815 A CN 106391815A
Authority
CN
China
Prior art keywords
die
preform
wall thickness
drawing part
blank
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610952055.1A
Other languages
Chinese (zh)
Inventor
汤泽军
杜浩
陶克梅
江双双
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nanjing University of Aeronautics and Astronautics
Original Assignee
Nanjing University of Aeronautics and Astronautics
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nanjing University of Aeronautics and Astronautics filed Critical Nanjing University of Aeronautics and Astronautics
Priority to CN201610952055.1A priority Critical patent/CN106391815A/en
Publication of CN106391815A publication Critical patent/CN106391815A/en
Pending legal-status Critical Current

Abstract

The invention discloses a device for improving uniformity of the wall thickness of a stamping deep drawing part. The device comprises a lower die base and an upper slide block; a female die base is connected to the upper end of the lower die base; a connection plate is connected to the lower end of the upper slide block; a performing male die and a performing female die are arranged in the middle of the position between the female die base and the connection plate; the performing male die is arranged at the lower end of the connection plate; and the performing female die is arranged in a cavity of the female die base. The invention further discloses a method for improving the uniformity of the wall thickness of the stamping deep drawing part. By means of the method, a blank is provided with preliminary convex parts or preliminary concave parts with certain heights and shapes, the material storing effect and the stress distribution effect which are achieved by performing play a role in improving the distribution uniformity of the wall thickness of the stamping deep drawing part during final barrel-shaped piece deep drawing; and in addition, the method has the advantages that the device is simple, multi-pass deep drawing procedures and tedious annealing procedures are not needed, the production cost is low, and the process is easy to adjust and control.

Description

A kind of device and method improving punching press drawing part evenness of wall thickness
Technical field
The invention belongs to punching press deep-drawing technique field, it is especially a kind of device improving punching press drawing part evenness of wall thickness And method.
Background technology
Drawing is exactly substantially the material of blank flange portion gradually to be transferred to the process of barrel, during transfer The material of flange, due to being acted on by drawing pressure, produces tension in radial direction, and produces compressive stress in circumference.In tension and Under the collective effect of compressive stress, the metal of flange portion produces plastic deformation, and constantly flows in die and become cylindrical member, due to Barrel material thickness under action of pulling stress is thinning, and the thickness of barrel material presents the trend of from top to bottom more and more thinner, and At cylinder bottom, fillet part thickness is the thinnest.Be gradually increased with drawing depth, finally cylinder bottom fillet position cracking so that The drawing depth shaping eventually is restricted.And due to localized necking, it is even to result in whole cylindrical member wall unevenness, cylinder bottom fillet Position relatively thin thus reduce its use during intensity.
In order to make up the intensity decreases brought by wall thickness reduction, need to increase overall wall thickness, and after this is produced Fruit is exactly that part quality increases, and this commercial production theory with current energy-conservation loss of weight is disagreed, for needing by mitigation vehicle body Weight and reaching reduce particularly important for the automobile industry that consumption of petroleum and greenhouse gas emission are target, simultaneously for For aerospace field, the loss of weight of parts is always the target of researcher struggle.For this reason, production work persons are to carry The evenness of wall thickness of high punching press drawing part have also been made many researchs.
In existing technology, for example, the patent of Zhang Yu(CN204135174U)In describe a kind of aluminum cylindrical member local The method thickening base, with pre- drawing die and partial thickening upsetting squeeze mould, using larger drawing gap, first passes through drawing Mould obtains the preform of certain depth and shape, then application upsetting squeeze mould by preform punch and kicker work Increased by the local that material is realized in upsetting squeeze with lower, therefore obtain the aluminum blank of Varying-thickness distribution, that is, in advance in drawing stress The thickness local of material at this is increased, so in drawing process on blank corresponding to the big and thinning serious region of thickness In, still there is enough material thick, thus avoiding ftractureing after material of partial thickening is thinning under action of pulling stress at this.This kind of Blank-making method is there is problems that need the strict depth controlling prefabricated blank, if dealing with improperly easily during follow-up upsetting squeeze Lead to the folding of plate due to Compressional buckling, and upsetting squeeze process convex mould has higher wanting with the routing motion of kicker Ask, otherwise just cannot obtain Varying-thickness base.
Chen Tan and et al. patent(CN103801608A)In describe a kind of not thinning deep-drawing technique of little flange cylindrical member, The feature of this patent is that the heating and softening that first blank of drawing is carried out with material is processed, and carries out specific acid to blank Property solution washing and surface embrocate lubricating oil, it is right to need after carrying out the deep-drawing technique of multi-pass and every time drawing afterwards Drawing part is made annealing treatment.There is the defects such as early stage blank preparatory process is relatively complicated in the method, can not enter for some For the material of row heat treated, this technique should not use.
The patent of Chen Baoguo et al.(CN105081045A)In describe a kind of sheet metal component hydro-mechanical drawing of homogenization deformation Manufacturing process, the feature of this patent is to be filled with liquid from the top of plate first, when making plate that plastic deformation, one section of pressurize to occur Between, positive bulging goes out the performing member of certain altitude, and removal upper liquid is passed through into concave die cavity and has certain pressure afterwards Liquid, makes performing member that plastic deformation occurs in the presence of punch, discharges the liquid of concave die cavity, so that panel beating is equal simultaneously Homogenize deformation.The method is there is problems that be difficult to be accurately controlled preform by fluid pressure highly and descending in punch During need between the descending amount of precise control punch and the decrement of concave die cavity liquid relation, because performing member leads to Cross bulging process to obtain, therefore performing member has had a certain amount of thinning, and the sealing to mould in whole forming process Property has higher requirements, and production cost is too high.
The eighties in 20th century, the method referred in topping up it is proposed that anti-inflation hydro-mechanical drawing is industrial on the basis of hydro-mechanical drawing Under the initial pressure effect of room fluid media (medium), there is bulging in sheet material, and obtain reservation shape by the constraint of mould, afterwards one Determine under liquid chamber pressure plate and carry out with punch motion that liquid filling deep-drawing forming is in opposite direction, it is attached that larger pre- bulk is easily caused die mouth Nearly folding of material, leads to part forming failure, thus limiting deflection and the performance of part, meanwhile, at preform and end In forming process, the sealing of mould is had higher requirements, this will increase the manufacturing cost of mould processing.
Therefore, a kind of new technique improving punching press drawing part evenness of wall thickness of exploitation, can make up all in prior art As higher in punch and kicker motion quality of fit, the defect such as operation is excessively loaded down with trivial details, can solve the problem that punching press drawing part wall thickness subtracts again Thin serious problem, breaks through the restriction of drawing depth in traditional deep-drawing technique, and the use intensity improving drawing cylindrical member has depth Remote meaning.
Content of the invention
For problems of the prior art, the invention discloses a kind of dress improving punching press drawing part evenness of wall thickness Put and method, the biscuit area corresponding to specifically at the cylinder bottom fillet position of thinning most serious is made preform and processed, and to improve A kind of technique of punching press drawing part evenness of wall thickness;The method of the present invention have equipment simple it is not necessary to the drawing work of multi-pass The advantages of sequence and loaded down with trivial details annealing operation, low production cost, process can easily be accommodated and control.
The present invention is realized in:A kind of device improving punching press drawing part evenness of wall thickness, including die shoe and Top shoe;The upper end of die shoe is connected with die pedestal;Top shoe lower end is connected with connecting plate;Described die pedestal and company Centre position between fishplate bar is provided with preform punch and preform die;Described preform punch is arranged on connecting plate Lower end;Described preform die is arranged in the die cavity of die pedestal;By piece pre-forming die(Preform punch and pre- Female die for forming)Preparation contains given shape, forms annular protrusion in corresponding cylindrical member fillet position, prefabricated blank part carries out tubular Part drawing shapes the evenness of wall thickness of cylindrical member to improve.
Further, described preform die is the preform die of rigid or the preform of flexible material is recessed Mould.
Further, described preform punch is dismountable, and with connecting plate interference fits.
Further, the upper end of described die pedestal is connected with preform blank holder.
Further, described preform blank holder is connected with die pedestal by soket head cap screw.
Further, two side positions between described die pedestal and connecting plate are also associated with guide pillar.
Further, the described upper end of described guide pillar is connected with the guide pin bushing in connecting plate;The lower end of described guide pillar It is fixed on die pedestal.
The invention also discloses a kind of method improving punching press drawing part evenness of wall thickness, comprise the following steps that:
(1)According to the physical dimension of final cylindrical member, calculate the blank of suitable size, and the table in blank and contacting dies Face coating lubricating oil;
(2)It is placed in die pedestal using preform die, blank is placed in preform die, will be pre- by soket head cap screw Shape blank holder to be connected with die pedestal;
(3)Start hydraulic press, so that blank forms pre- projection in the presence of preform punch and preform die;Reach During preform height, preform punch travel terminates, prepared preform blank;Shaped with storing effect by preform die Should be with the preform blank improving stress distribution effect;
(4)Using whole shaping dies, that is, change preform punch, preform die and preform blank holder, change whole shaping into Punch, whole female die for forming and whole shaping blank holder, by the pre- projection of preform blank, upward or pre- projection is installed on end down In female die for forming, and position-limiting action is played by spacing annulus.
(5)It is uniformly distributed Rectangular Spring shaping blank holder eventually, by the bolt being connected with die base threaded bore, screw in Nut;Screw in nut and produce certain precompressed amount and then produce spring force, thus providing suitable plate pressure-pad-force;By equal Cloth is shaping the certain decrement of the Rectangular Spring generation on blank holder to provide plate pressure-pad-force eventually;
(6)Restart in hydraulic press, whole forming terrace die is descending, make preform plate plastic deformation occur, in whole forming terrace die Descending reach setting height when, shape eventually and terminate, take out the punching press drawing part of uniform wall thickness.
Further, described preform die is the preform die of rigid or the preform of flexible material is recessed Mould.
The contemplated technical scheme of the present invention compared with prior art, has the advantages that:
(1) of the present invention is traditional punching press cupping tool it is not necessary to the highly sophisticated device of other auxiliary, decreases and sets Standby investment and production cost.
(2) do not need previously prepared go out the blank of Varying-thickness and preparation process in need strictly to limit the depth of prefabricated blank The problems such as with the folding of plate being led to due to extruding unstability during upsetting squeeze.And do not need higher routing motion precision.
(3) present invention only need to preform and eventually shape twice drawing sequence it is not necessary to the drawing sequence of multi-pass and Loaded down with trivial details annealing operation, it is to avoid the problems such as thus produced processing cost is too high, and, the present invention is also suitable some can not Carry out the material of heat treated.
(4) the preform plate with storing effect and stress distribution effect obtained by preform of the present invention, at end The effect that feed supplement can be played during shaping and change thinning critical regions stress state, can be effectively improved punching press drawing part wall thickness The uniformity of distribution.
Brief description
Fig. 1 is the piece pre-forming die assembling schematic diagram adopting rigid in the embodiment of the present invention 1.
Fig. 2 is the close-up schematic view of plate and rigid matrix contact site during preform in the embodiment of the present invention 1.
Fig. 3 is whole shaping dies assembling schematic diagram in the embodiment of the present invention 1.
Fig. 4 is whole forming terrace die and plate initial position close-up schematic view in the embodiment of the present invention 1.
Fig. 5 is the experimental result obtained in the embodiment of the present invention 2.
Fig. 6 is the piece pre-forming die assembling schematic diagram adopting flexible material in the embodiment of the present invention 2.
Fig. 7 is that during preform in the embodiment of the present invention 2, plate and the partial enlargement of flexible preform die contact site show It is intended to.
Fig. 8 is whole shaping dies assembling schematic diagram in the embodiment of the present invention 2.
Fig. 9 is whole forming terrace die and plate initial position close-up schematic view in the embodiment of the present invention 2.
Wherein, 1- die shoe, 2- die pedestal, 3- guide pillar, 4- preform blank holder, 5- guide pin bushing, 6- connecting plate is sliding on 7- Block, 8- preform punch, 9- blank, 10- preform die.
Specific embodiment
In order that the purpose of the present invention, technical scheme, implementation steps and advantages of the present invention are more specific understanding, once Elaborate in conjunction with accompanying drawing, embodiment and experimental data.It should be appreciated that specific embodiment described herein is only in order to solve Release the present invention, be not intended to limit the present invention, represent at I in accompanying drawing is at the partial enlargement of the present invention.
Embodiment 1
According to the design of the present invention, the preform blank with necessarily pre- convex shape should be prepared first.As shown in Figure 1 and 2, Preform blank is shaped using the piece pre-forming die of this rigid, it specifically includes following steps:
(1)According to the physical dimension of final cylindrical member, calculate suitable size blank 9, and the table in blank 9 and contacting dies Face coating lubricating oil.And blank 9 is placed in the preform die 10 of rigid;By having, necessarily pre- raised rigidity is pre- Female die for forming 10 is fixed in the die cavity in die pedestal 2.
(2)By soket head cap screw, preform blank holder 4 is connected with die pedestal 2, original plate is played with flanging and makees With.Preform punch 8 is designed to detachable, its with connecting plate 6 interference fits, during preform punch 8 down stroke, It is play the guiding role by the guide pillar 3 and the guide pin bushing 5 in connecting plate 6 being fixed in die pedestal 2.
(3)Start hydraulic press, top shoe 7 drives connecting plate 6 to move downward, and preform punch 8 is contacted with plate 9, makes plate Material 9 is contacted with the preform die 10 of rigid and deforms, and in the presence of preform punch, plate occurs plasticity to become Shape, when preform goes out to have the pre- projection preform punch of certain altitude and shape and goes downwards to certain distance, preform punch row Journey terminates, and unloads plate preform blank holder 4, takes out preform blank 9.Preform blank obtained by preform has necessarily Height and the pre- projection of definite shape, it changes the effect of blank stress distribution, such as Fig. 3 when having storing effect and shaping eventually Shown, shown is whole shaping dies assembling schematic diagram in the present embodiment, namely preform blank formal dress (pre- projection is upward) mould Tool schematic diagram;
(4)On the basis of preform mould bases, take off the detachably pre- of blank holder in piece pre-forming die and forced connection Forming terrace die, changes whole forming terrace die.In die pedestal 2, put into whole female die for forming, preform blank 9 formal dress is fixed on In whole female die for forming, as shown in Fig. 4 whole forming terrace die and plate initial relative position close-up schematic view.
(5)Install after shaping blank holder eventually, eight are evenly distributed on the bolt screw-in shaping on blank holder eventually recessed In the screwed hole of mold base, in each bolt, pack into a Rectangular Spring, make spring produce one by screwing in the nut of end Fixed decrement, thus provide shape required plate pressure-pad-force eventually.
(6)During whole forming terrace die is descending, by being fixed on the guide pin bushing 5 in guide pillar 3 and connecting plate 6 in die matrix 2 It play the guiding role.
(7)Start hydraulic press, upper slide 7 drives connecting plate 6 to move downward, make preform plate that plastic deformation to occur, When whole forming terrace die goes downwards to setpoint distance, shape eventually and terminate, take out the punching press drawing part of uniform wall thickness.
Embodiment 2
As shown in Fig. 6 ~ 7, the piece pre-forming die of the flexible material of employing prepares the preform with necessarily pre- convex shape Material, it specifically includes following steps:
1)According to the physical dimension of final cylindrical member, calculate suitable size blank 9, and the table in blank 9 and contacting dies Face coating lubricating oil.And blank 9 is placed in the preform die 10 of flexible material.The preform die 10 of flexible material, The such as flexibility such as polyurethane rubber, natural rubber rod, silica gel stick soft mode, the preform die 10 of flexible material is fixed on In die cavity in die pedestal 2.
2)By soket head cap screw, preform blank holder 4 is connected with die pedestal 2, original plate is played with flanging and makees With.Preform punch 8 is designed to detachable, it during preform punch 8 down stroke, is led to connecting plate 6 interference fits Cross the guide pillar 3 being fixed in die pedestal 2 to play the guiding role with the guide pin bushing 5 in connecting plate 6.
3)Start hydraulic press, top shoe 7 drives connecting plate 6 to move downward, and preform punch 8 is contacted with plate 9, makes plate 9 are deformed with the preform die 10 of flexible material, and due to the Incoercibility of rubber type of material, and it is limited to and has In the container of constant volume, under external force, according to law of minimum resistance, rubber type of material will move upwards, pushing plate Material, in the presence of rubber power, there is plastic deformation in plate, and preform goes out to have the pre- projection of certain altitude and shape, preformation When shape punch reaches setting height, preform punch travel terminates, and unloads plate preform blank holder 4 and takes out preform blank 9. Preform blank obtained by preform has the pre- projection of certain altitude and definite shape, and it has storing effect and becomes eventually Change the effect of blank stress distribution, as shown in figure 8, being whole shaping dies assembling schematic diagram in the present embodiment, namely in advance during shape Forming blank is counter to fill (pre- projection is down) mould schematic diagram;
4)On the basis of preform mould bases, that takes off preform blank holder 4 in piece pre-forming die and forced connection can Dismounting preform punch 8, changes whole forming terrace die.In die pedestal 2, put into whole female die for forming, fill counter for preform blank 9 It is fixed in whole female die for forming, as shown in Fig. 9 whole forming terrace die and plate initial relative position close-up schematic view.
5)Install after shaping blank holder eventually, eight are evenly distributed on the bolt shaping eventually on blank holder and screw in die In the screwed hole of pedestal, in each bolt, pack into a Rectangular Spring, so that spring is produced necessarily by screwing in the nut of end Decrement, thus provide shaping eventually required plate pressure-pad-force.
6)During whole forming terrace die is descending, by being fixed on the guide pin bushing 5 in guide pillar 3 and connecting plate 6 in die matrix 2 Guide effect.
7)Start hydraulic press, upper slide 7 drives connecting plate 6 to move downward, make preform plate plastic deformation occur, at end When forming terrace die goes downwards to setpoint distance, shape eventually and terminate, take out the punching press drawing part of uniform wall thickness.
Carry out a series of experimental verification for the present embodiment, we have been carried out at preform to original plate respectively Reason, preform convex mould diameter is respectively 12mm, 16mm, 20mm, and the preform slab height of every group of situation is 2mm, laggard Row cylindrical member shapes eventually, and the height of drawing is 11mm, for the ease of comparing, has carried out traditional Cup drawing and has obtained drawing Test specimen, obtains cylindrical member Thickness Distribution as shown in figure 5, tubular knowable to the experimental data obtaining, obtained by three kinds of preforms Cylindrical member obtained by the more direct drawing of the Reducing thickness at punch-nose angle for the part is less at punch-nose angle, and, with preformation The increase of shape convex mould diameter, the reduction at punch-nose angle is with minimizing that is to say, that evenness of wall thickness is more preferable.Directly drawing When, the reduction at punch-nose angle is 29%;During a diameter of 12mm of preform, the reduction at punch-nose angle is 26%;Preform During a diameter of 16mm, the reduction at punch-nose angle is 22%;During a diameter of 20mm of preform, the reduction at punch-nose angle is 12%, if using the intensity at the punch-nose angle of most serious thinning during direct drawing as limiting safe load, using preform The cylindrical member obtaining thickness when meeting intensity requirement can reduce 17%, and for the automobile panel of area one timing, quality will Reduce 17%, this is for being to be considerable for the automobile industry of target at this stage to mitigate weight.As described above, experiment Result confirms that the present invention can be obviously improved punching press drawing part evenness of wall thickness.
As it will be easily appreciated by one skilled in the art that the foregoing is only the preferable enforcement row of the present invention, it is not used to Limit the present invention, all any modification, equivalent and improvement made within the spirit and principles in the present invention, all should include In protection scope of the present invention.

Claims (9)

1. a kind of device improving punching press drawing part evenness of wall thickness, including die shoe(1)And top shoe(7);Die shoe(1) Upper end be connected with die pedestal(2);Top shoe(7)Lower end is connected with connecting plate(6)It is characterised in that described die base Seat(2)And connecting plate(6)Between centre position be provided with preform punch(8)And preform die(10);Described Preform punch(8)It is arranged on connecting plate(6)Lower end;Described preform die(10)It is arranged on die pedestal(2)Type In chamber.
2. the device improving punching press drawing part evenness of wall thickness according to claim 1 is it is characterised in that described preformation Shape die(10)Preform die for rigid or the preform die of flexible material.
3. the device improving punching press drawing part evenness of wall thickness according to claim 1 is it is characterised in that described preformation Shape punch(8)It is dismountable, and and connecting plate(6)Interference fits.
4. the device improving punching press drawing part evenness of wall thickness according to claim 1 is it is characterised in that described die Pedestal(2)Upper end be connected with preform blank holder(4).
5. the device improving punching press drawing part evenness of wall thickness according to claim 4 is it is characterised in that described preformation Shape blank holder(4)By soket head cap screw and die pedestal(2)Connect.
6. the device improving punching press drawing part evenness of wall thickness according to claim 1 is it is characterised in that described die Base(2)And connecting plate(6)Between two side positions be also associated with guide pillar(3).
7. the device improving punching press drawing part evenness of wall thickness according to claim 6 is it is characterised in that described is described Guide pillar(3)Upper end and connecting plate(6)In guide pin bushing(5)It is connected;Described guide pillar(3)Lower end be fixed on die pedestal (2).
8. a kind of method improving punching press drawing part evenness of wall thickness is it is characterised in that step is as follows:
1)Calculate the blank mating with the physical dimension of final cylindrical member(9);
2)Using piece pre-forming die, by preform die(10)It is placed in die pedestal(2)In, by blank(9)It is placed in preform recessed Mould(10)In, by soket head cap screw by preform blank holder(4)With die pedestal(2)Connect;
3)Start hydraulic press, in preform punch(8)And preform die(10)In the presence of so that blank(9)Formed pre- Raised;When reaching preform height, preform punch travel terminates, prepared preform blank;
4)Using whole shaping dies, that is, replace preform punch(8), preform die(10)And preform blank holder(4), By the pre- projection of preform blank, upward or pre- projection is installed in whole female die for forming down;
5)Be uniformly distributed spring shaping eventually blank holder, by with die pedestal(2)The bolt that screwed hole is connected, screws in nut;
6)Restart in hydraulic press, whole forming terrace die is descending, make preform plate plastic deformation occur, under whole forming terrace die When row reaches the height of setting, shape eventually and terminate, take out the punching press drawing part of uniform wall thickness.
9. the method improving punching press drawing part evenness of wall thickness according to claim 8 is it is characterised in that described preformation Shape die(10)Preform die for rigid or the preform die of flexible material.
CN201610952055.1A 2016-11-03 2016-11-03 Device and method for improving uniformity of wall thickness of stamping deep drawing part Pending CN106391815A (en)