CN106281011A - A kind of cationic wax emulsion for leather finish and preparation method thereof - Google Patents
A kind of cationic wax emulsion for leather finish and preparation method thereof Download PDFInfo
- Publication number
- CN106281011A CN106281011A CN201610801124.9A CN201610801124A CN106281011A CN 106281011 A CN106281011 A CN 106281011A CN 201610801124 A CN201610801124 A CN 201610801124A CN 106281011 A CN106281011 A CN 106281011A
- Authority
- CN
- China
- Prior art keywords
- parts
- wax emulsion
- wax
- leather
- water
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a kind of cationic wax emulsion for leather finish and preparation method thereof, belonging to wax emulsion preparing technical field, this wax emulsion is made up of the raw material of following weight portion: 0.5 3.5 parts of Cera Flava, dodecyl dimethyl benzyl ammonium chloride 0.9 3.2 parts, positive eicosanol 14 parts, chlorinated paraffin 26 parts, 3 10 parts of ant wax, dibenzyl cumenyl phenol polyethenoxy ether 1.2 5 parts, Xanthan gum 0.5 3 parts and 80 170 parts of water.The cationic wax emulsion for leather finish that the present invention provides can improve feel and the resistance to water of leather finishing agent, and real leather products feel can be made more excellent, and it can reach preferable underseal effect after leather primary coat simultaneously.
Description
Technical field
The present invention relates to the preparation method of a kind of wax emulsion, particularly to a kind of leather finish cationic wax emulsion and
Its preparation method.
Background technology
Wax emulsion in leather industry mainly as leather finish auxiliary agent, for the end, in, top coat, there is preferable performance.
Wax had both had the general character of water proofing property and lubricity, in terms of having again such as oiliness, viscosity, fragility, toughness, fusibleness and gloss
Characteristic, is very different to each other.In actual applications, a kind of wax can not have the institute met required for a certain special-purpose
There is character.Therefore, when selecting the raw material of leather finish wax emulsion, the serviceability of wax to be considered, improves leather and is coated with
The Spraying technique of decorations.According to the type of emulsifying agent used, wax emulsion is often divided into anionic, nonionic, cationic and two
Property ion-type four class.Owing to generally showing elecrtonegativity without the skin base surface covered with paint, lacquer, colour wash, etc., can be relatively covering with paint, lacquer, colour wash, etc. processing cationic wax emulsion
Soon combined with leather surface and form thin film, it is effectively prevented coating material too much permeation effects leather hand feeling, makes skin
Leather embodies the performances such as good, the elegant softness of feel of coat fastness.Based on above advantage, cationic wax emulsion is subject to the most more and more
To researcher and the favor of user, abroad to its research and development the most for many years, and define numerous in variety, excellent performance
Tandem product.
Chinese patent application CN101585968 discloses cationic wax emulsion and the preparation thereof of a kind of used in leather processing procedure
Method: it is made up of following raw materials according: Brazil wax, OP wax, dimethicone, hexadecanol, lipophilic emulsifier compound system,
Hydrophilic emulsifier compound system, 1631 cationic surfactants.Although this cationic wax emulsion has good stability, water and milk
The advantages such as good, the environmental protection of the property changed, but its feel after leather bottom is covered with paint, lacquer, colour wash, etc. is the most puckery, and wax sense is not strong, on the other hand as underseal
Wax emulsion, the permeability of its emulsion is too strong, easily causes moist feeling, have impact on the quality of leather after covering with paint, lacquer, colour wash, etc. leather.
Summary of the invention
It is an object of the invention to overcome in prior art the wax sense existing for leather primary coat cationic wax emulsion strong,
The deficiency that astringent sense is heavier, it is provided that a kind of cationic wax emulsion for leather finish and preparation method thereof.This wax emulsion can be used
In improving feel and the resistance to water of leather finishing agent, real leather products feel can be made more excellent.
In order to realize foregoing invention purpose, the invention provides techniques below scheme:
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following weight portion: Cera Flava 0.5-3.5 part,
Dodecyl dimethyl benzyl ammonium chloride 0.9-3.2 part, positive eicosanol 1-4 part, chlorinated paraffin 2-6 part, ant wax 3-10 part, two
Benzyl cumenyl phenol polyethenoxy ether 1.2-5 part, Xanthan gum 0.5-3 part and water 80-170 part.
Preferably, a kind of cationic wax emulsion for leather finish, it is made up of the raw material of following weight portion: Cera Flava 0.6-
3.2 parts, dodecyl dimethyl benzyl ammonium chloride 1-3 part, positive eicosanol 1.1-3.5 part, chlorinated paraffin 2.2-5.4 part, ant
Wax 4-9 part, dibenzyl cumenyl phenol polyethenoxy ether 1.5-4.7 part, Xanthan gum 0.7-2.8 part and water 90-160 part.
It is furthermore preferred that a kind of cationic wax emulsion for leather finish, it is made up of the raw material of following weight portion: Cera Flava
0.8-2.6 part, dodecyl dimethyl benzyl ammonium chloride 1.2-2.8 part, positive eicosanol 1.3-3.2 part, chlorinated paraffin 2.5-5
Part, ant wax 5-8 part, dibenzyl cumenyl phenol polyethenoxy ether 1.7-4.5 part, Xanthan gum 0.9-2.5 part and water 115-150
Part.
Most preferably, a kind of cationic wax emulsion for leather finish, it is made up of the raw material of following parts by weight: Cera Flava
2.4 parts, dodecyl dimethyl benzyl ammonium chloride 1.7 parts, positive eicosanol 2.5 parts, chlorinated paraffin 4.5 parts, 7 parts of ant wax, two
Benzyl cumenyl phenol polyethenoxy ether 2.6 parts, Xanthan gum 1.7 parts and 140 parts of water.
Another object of the present invention is to provide the preparation method of a kind of cationic wax emulsion for leather finish, including
Following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 in homogenizer
Carbon alcohol, is heated to 70-80 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 65-75 DEG C, obtains Aqueous dispersions mixing
Thing;
S3 improves the mixing speed of homogenizer and enters to 2000-3000rpm, Aqueous dispersions mixture prepared by addition step S2
Row emulsifying, emulsification times is 1-3h;Decline in the mixing speed that speed is 200-300rpm subsequently and warm to room temperature, add xanthic acid
Continue stirring 10-30min after glue, be then filtrated to get leather finish wax emulsion.
Preferably, in above-mentioned steps S3, the mesh number of filtration filter screen is 100-200 mesh.
Compared with prior art, beneficial effects of the present invention:
The cationic wax emulsion for leather finish that the present invention provides can improve the feel of leather finishing agent and water-fast
Property, real leather products feel can be made more excellent, it can reach preferable underseal effect after leather primary coat simultaneously.
Detailed description of the invention
Below in conjunction with test example and detailed description of the invention, the present invention is described in further detail.But this should not understood
Scope for the above-mentioned theme of the present invention is only limitted to below example, and all technology realized based on present invention belong to this
The scope of invention.
Embodiment 1
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following parts by weight: 2.4 parts of Cera Flava, ten
Dialkyl dimethyl benzyl ammonium chloride 1.7 parts, positive eicosanol 2.5 parts, chlorinated paraffin 4.5 parts, 7 parts of ant wax, dibenzyl isopropyl
Phenyl phenol polyoxyethylene ether 2.6 parts, Xanthan gum 1.7 parts and 140 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 in homogenizer
Carbon alcohol, is heated to 70 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 2000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 2h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 200 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 12.3%, PH:5.1, product stability, 50
DEG C, within three months, outward appearance is unchanged.
Embodiment 2
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following parts by weight: 0.5 part of Cera Flava, ten
Dialkyl dimethyl benzyl ammonium chloride 0.9 part, positive eicosanol 4 parts, chlorinated paraffin 2 parts, 10 parts of ant wax, dibenzyl cumenyl
Phenol polyethenoxy ether 5 parts, Xanthan gum 3 parts and 170 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 in homogenizer
Carbon alcohol, is heated to 70 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 3000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 1h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 150 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 10.1%, PH:5.65, product stability, 50
DEG C, within three months, outward appearance is unchanged.
Embodiment 3
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following weight portion: 3.5 parts of Cera Flava, 12
Zephiran 3.2 parts, positive eicosanol 1 part, chlorinated paraffin 6 parts, 3 parts of ant wax, dibenzyl cumenyl phenol
Polyoxyethylene ether 1.2 parts, Xanthan gum 0.5 part and 80 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 in homogenizer
Carbon alcohol, is heated to 80 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 3000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 1h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 150 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 18.7%, PH:4.92, product stability, 50
DEG C, within three months, outward appearance is unchanged.
Embodiment 4
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following weight portion: 2 parts of Cera Flava, dodecane
Base dimethyl benzyl ammonium chloride 1.9 parts, positive eicosanol 3 parts, chlorinated paraffin 4 parts, 6 parts of ant wax, dibenzyl cumenyl phenol are poly-
Oxygen vinyl Ether 3.6 parts, Xanthan gum 2.1 parts and 135 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 in homogenizer
Carbon alcohol, is heated to 70 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 3000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 1h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 150 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 11.5%, PH:5.0, product stability, 50
DEG C, within three months, outward appearance is unchanged.
Comparative example 1
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following parts by weight: 2.4 parts of Cera Flava, ten
Dialkyl dimethyl benzyl ammonium chloride 1.7 parts, positive eicosanol 2.5 parts, chlorinated paraffin 4.5 parts, dibenzyl cumenyl phenol are poly-
Oxygen vinyl Ether 2.6 parts, Xanthan gum 1.7 parts and 140 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, chlorinated paraffin, dibenzyl cumenyl phenol polyethenoxy ether and positive eicosanol in homogenizer,
It is heated to 70 DEG C to melt, stirs, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 2000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 2h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 200 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 12%, PH:5.1, product stability, 50 DEG C,
Within three months, outward appearance is unchanged.
Comparative example 2
A kind of cationic wax emulsion for leather finish, is made up of the raw material of following parts by weight: 2.4 parts of Cera Flava, ten
Dialkyl dimethyl benzyl ammonium chloride 1.7 parts, positive eicosanol 2.5 parts, 7 parts of ant wax, dibenzyl cumenyl phenol polyethenoxy
2.6 parts of ether, Xanthan gum 1.7 parts and 140 parts of water.
The preparation method of above-mentioned cationic wax emulsion, comprises the following steps:
S1 adds Cera Flava, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive eicosanol, heating in homogenizer
Melt to 70 DEG C, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 2000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 2h;Decline in the mixing speed that speed is 200rpm subsequently and warm to room temperature, continue to stir after adding Xanthan gum
Mix 20min, be then filtrated to get leather finish cationic wax emulsion via 200 mesh filter screens.
Cationic wax emulsion performance indications: faint yellow emulsion, solid content 11.7%, PH:5.2, product stability, 50
DEG C, within three months, outward appearance is unchanged.
Wax emulsion embodiment 1-4 prepared is deployed into slurry by primary coat formula consumption and primary coat acrylic emulsion, is coated with
After decorations Corii Bovis seu Bubali leather, leather hand feeling is full, gentle, and wax sense is strong, has the resistance to water of excellence simultaneously.And the wax breast of comparative example 1 preparation
After liquid is deployed into slurry in same application formula ratio ratio, after covering with paint, lacquer, colour wash, etc. Corii Bovis seu Bubali leather, leather hand feeling is poor, and wax sense is weak, and astringent sense is heavier.
And after the wax emulsion of comparative example 2 preparation is deployed into slurry, after covering with paint, lacquer, colour wash, etc. Corii Bovis seu Bubali leather, leather exist wax sense weak while the asking of poor water resistance
Topic.
Claims (6)
1. the wax emulsion for leather finish, it is characterised in that be made up of the raw material of following weight portion: Cera Flava 0.5-3.5
Part, dodecyl dimethyl benzyl ammonium chloride 0.9-3.2 part, positive eicosanol 1-4 part, chlorinated paraffin 2-6 part, ant wax 3-10
Part, dibenzyl cumenyl phenol polyethenoxy ether 1.2-5 part, Xanthan gum 0.5-3 part and water 80-170 part.
Wax emulsion for leather finish the most according to claim 1, it is characterised in that by the raw material system of following weight portion
Become: Cera Flava 0.6-3.2 part, dodecyl dimethyl benzyl ammonium chloride 1-3 part, positive eicosanol 1.1-3.5 part, chlorinated paraffin
2.2-5.4 part, ant wax 4-9 part, dibenzyl cumenyl phenol polyethenoxy ether 1.5-4.7 part, Xanthan gum 0.7-2.8 part and water
90-160 part.
Wax emulsion for leather finish the most according to claim 2, it is characterised in that by the raw material system of following weight portion
Become: Cera Flava 0.8-2.6 part, dodecyl dimethyl benzyl ammonium chloride 1.2-2.8 part, positive eicosanol 1.3-3.2 part, chlorination stone
Wax 2.5-5 part, ant wax 5-8 part, dibenzyl cumenyl phenol polyethenoxy ether 1.7-4.5 part, Xanthan gum 0.9-2.5 part and water
115-150 part.
Wax emulsion for leather finish the most according to claim 3, it is characterised in that by the raw material of following parts by weight
Make: 2.4 parts of Cera Flava, dodecyl dimethyl benzyl ammonium chloride 1.7 parts, positive eicosanol 2.5 parts, chlorinated paraffin 4.5 parts, ant
7 parts of wax, dibenzyl cumenyl phenol polyethenoxy ether 2.6 parts, Xanthan gum 1.7 parts and 140 parts of water.
5. according to the preparation method of the wax emulsion for leather finish described in any one of claim 1-4, it is characterised in that bag
Include following steps:
S1 adds Cera Flava, chlorinated paraffin, ant wax, dibenzyl cumenyl phenol polyethenoxy ether and positive 20 carbon in homogenizer
Alcohol, is heated to 70-80 DEG C and melts, stir, obtain oil phase dispersed mixture;
S2 is soluble in water by dodecyl dimethyl benzyl ammonium chloride, is heated to 65-75 DEG C, obtains Aqueous dispersions mixture;
S3 improves the mixing speed of homogenizer and carries out breast to 2000-3000rpm, Aqueous dispersions mixture prepared by addition step S2
Changing, emulsification times is 1-3h;Decline in the mixing speed that speed is 200-300rpm subsequently and warm to room temperature, after adding Xanthan gum
Continue stirring 10-30min, be then filtrated to get leather finish wax emulsion.
The preparation method of the wax emulsion for leather finish the most according to claim 5, it is characterised in that described step S3
Described in the mesh number of filtration filter screen be 100-200 mesh.