CN106278072A - A kind of method without soil tailings - Google Patents
A kind of method without soil tailings Download PDFInfo
- Publication number
- CN106278072A CN106278072A CN201610669372.2A CN201610669372A CN106278072A CN 106278072 A CN106278072 A CN 106278072A CN 201610669372 A CN201610669372 A CN 201610669372A CN 106278072 A CN106278072 A CN 106278072A
- Authority
- CN
- China
- Prior art keywords
- soil
- tailings
- mine tailing
- low
- coombe
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention provides a kind of method without soil tailings, including Tailing thickening, filling subsidence area, coombe, low-lying land, preparation is without soil mine tailing substrate with without steps such as soil mine tailing substrate coverings, it is possible not only to process a large amount of mine tailing, reduces mine tailing and take up an area, reduce environmental hazard, make resource of tailings obtain Appropriate application simultaneously, improve resource utilization.There is preferable economic benefit and social benefit.Obtained is high without soil mine tailing substrate machine matter content, and water-retaining property and good permeability can improve the physicochemical property of soil, it is provided that plant desired nutritional, repair mine and have preferable recovery dynatron effect.
Description
Technical field
The present invention relates to tailings glass field, be specifically related to a kind of method without soil tailings.
Background technology
Produce substantial amounts of mine tailing during mining, do not only take up substantial amounts of soil, cause to the ecological environment of surrounding
The biggest harm, and to put into process and maintenance cost.If mine tailing consolidation is filled to subsidence area, coombe, low-lying land are made
Ground, both can make full use of resource of tailings, turn waste into wealth, the subsidence area not utilized, coombe, low-lying land can be made again to reclaim into cultivated
Ground, forest land, meadow etc., improve land utilization ratio.
Generally requiring during mine reclamation and carry out soil moved in improve the original engineering, soil moved in improve the original can endanger taking soil reclamation soil fail
Its surrounding enviroment.If mine tailing in addition auxiliary material being made without soil mine tailing substrate, not only reducing soil moved in improve the original amount, also making resource of tailings
Obtain Appropriate application, improve resource utilization.At present, have not yet seen and both utilize mine tailing consolidation filling to make ground, use again simultaneously
Mine tailing is prepared soilless substrate covering and is made the report that surface layer carries out reclaiming.
Summary of the invention
In order to solve above technical problem, the present invention proposes a kind of method without soil tailings, and the method is applicable to ore deposit
Subsidence area, coombe or the low-lying land existed near mountain, specifically includes following steps:
(1) Tailing thickening
Concentrating selecting factory's new last person ore in sand form to send into Paste thickener together with flocculant, new last person's ore in sand form is by by institute
Dry tailings weight addition per ton described flocculant 95g~130g contained, water return pipeline is sent in the overflow that described concentrator produces
Recycle;
(2) the mastic tail of the underflow density 65%~70% that concentrator described in filling subsidence area, coombe, low-lying land produces
Ore deposit, filling subsidence area, coombe or low-lying land, then flatten;Specifically may comprise steps of:
Charging stirring: by described Paste tailings, slag cements by weight percent: Paste tailings 95%~97%, slag
Cement 3%~5%, adds agitator stirring 5min;
Consolidation filling: the stirring thing stirred is delivered to subsidence area, coombe or low-lying land heap row and consolidation;
Leveling: flatten through bull-dozer;
(3) preparation is without soil mine tailing substrate
Dispensing: according to percetage by weight: mine tailing 30%~40%, turfy soil 40%~50%, Vermiculitum 3%~5%, pumice
3%~5%, Maifanitum 3%~5%, decomposed manure 6%~10% are sufficiently mixed uniformly;Described Vermiculitum granularity is preferably 40
Mesh~60 mesh, described pumice granularity is preferably 60 mesh~80 mesh, and described Maifanitum granularity is preferably 60 mesh~80 mesh;
Ripening: ripening 5-8 days of being banked up by the material mixed, during banking up, remains the moisture of material
It is 40%~50%;
(4) cover without soil mine tailing substrate
Told subsidence area, coombe, low-lying land are filled, after leveling, cover its surface by described without soil mine tailing substrate, cover
Thickness is 25-35cm, then carries out vegetation and reclaims.
Described flocculant is made up of bodied ferric sulfate and polyacrylamide, and new last person's ore in sand form per ton adds described polyaluminum sulfate
Ferrum 80g~100g and described polyacrylamide 15g~30g.
Method without soil tailings provided by the present invention, consolidates mine tailing filling coombe, low-lying land and subsidence area and makes
Ground, and mine tailing is prepared as soilless substrate cover make surface layer, for substitute in the repair process of mine use soil moved in improve the original.The method
Not only process a large amount of mine tailing, reduced mine tailing and take up an area, reduce environmental hazard, make resource of tailings obtain Appropriate application simultaneously, improve
Resource utilization.There is preferable economic benefit and social benefit.Obtained is high without soil mine tailing substrate machine matter content, water-retaining property
And good permeability, the physicochemical property of soil can be improved, it is provided that plant desired nutritional, repair to have to mine and preferably repair effect
Should.
Detailed description of the invention:
Embodiment 1:
Iron ore mine, Dandong City of Liaoning Province, there is more coombe and low-lying land in mine periphery, uses without soil tailings side
Method, to coombe and low-lying land Reclamation by filling, comprises the following steps:
(1) Tailing thickening
Concentrating selecting factory new last person ore deposit to send into Paste thickener together with flocculant, flocculant addition is new row
CHARACTERISTICS OF TAILINGS SAND is by by contained dry tailings weight addition per ton bodied ferric sulfate 80g and polyacrylamide 30g.Concentrator overflow is sent
Enter water return pipeline to recycle;
(2) filling coombe, low-lying land
The Paste tailings of thickener underflow concentration 65%, for filling coombe, low-lying land, subsidence area, comprises the following steps:
Charging stirring: by Paste tailings, slag cements by weight percent: Paste tailings 95%, slag cements 5%, add
Enter agitator stirring 5min.
Consolidation filling: by belt conveyor, the Paste tailings stirred is delivered to coombe, low-lying land heap is arranged and consolidation.
Leveling: mine tailing is full of after drying up and flattens through bull-dozer.
(3) preparation is without soil mine tailing substrate
Comprise the following steps without soil mine tailing substrate:
Dispensing: according to percetage by weight: iron tailings 30%, turfy soil 50%, Vermiculitum 4%, pumice 3%, Maifanitum 3%,
Decomposed manure 10% is sufficiently mixed uniformly;
Ripening: ripening 7 days of being banked up by the material mixed, during banking up, remains that the moisture of material is
40%~50%.
(4) cover without soil mine tailing substrate
After coombe and low-lying land Paste tailings heap row are full of leveling, that is prepared by this mine tailing covers its table without soil mine tailing substrate
Face 30cm, then carries out vegetation and reclaims.
What the present embodiment was provided has not only processed a large amount of mine tailing without soil tailings method, reduces mine tailing and takes up an area, reduces
Environmental hazard, makes resource of tailings obtain Appropriate application simultaneously, improves resource utilization.There is preferable economic benefit and society's effect
Benefit.Obtained is high without soil mine tailing substrate machine matter content, and water-retaining property and good permeability can improve the physicochemical property of soil, it is provided that
Plant desired nutritional, repairs mine and has preferable recovery dynatron effect.
Embodiment 2:
Chaoyang City, Liaoning Province Molybdenum Mine, there is subsidence area in mine periphery, use without soil tailings method to coombe and
Low-lying land Reclamation by filling, comprises the following steps:
(1) Tailing thickening
Concentrating selecting factory new last person ore deposit to send into Paste thickener together with flocculant, flocculant addition is new row
CHARACTERISTICS OF TAILINGS SAND is by by contained dry tailings weight addition per ton bodied ferric sulfate 90g and polyacrylamide 22g.Concentrator overflow is sent
Enter water return pipeline to recycle;
(2) filling subsidence area
The Paste tailings of thickener underflow concentration 68%, for filling subsidence area, comprises the following steps:
Charging stirring: by Paste tailings, slag cements by weight percent: Paste tailings 96%, slag cements 4%, add
Enter agitator stirring 5min.
Consolidation filling: the Paste tailings stirred is delivered to subsidence area heap by belt conveyor and arranges and consolidation.
Leveling: mine tailing is full of after drying up and flattens through bull-dozer.
(3) preparation is without soil mine tailing substrate
Comprise the following steps without soil mine tailing substrate:
Dispensing: according to percetage by weight: molybdic tailing 35%, turfy soil 45%, Vermiculitum 3%, pumice 5%, Maifanitum 4%,
Decomposed manure 8% is sufficiently mixed uniformly;
Ripening: ripening 5 days of being banked up by the material mixed, during banking up, remains that the moisture of material is
40%~50%.
(4) cover without soil mine tailing substrate
After subsidence area Paste tailings heap row is full of leveling, that is prepared by this mine tailing covers its surface without soil mine tailing substrate
30cm, then carries out vegetation and reclaims.
What the present embodiment was provided has not only processed a large amount of mine tailing without soil tailings method, reduces mine tailing and takes up an area, reduces
Environmental hazard, makes resource of tailings obtain Appropriate application simultaneously, improves resource utilization.There is preferable economic benefit and society's effect
Benefit.Obtained is high without soil mine tailing substrate machine matter content, and water-retaining property and good permeability can improve the physicochemical property of soil, it is provided that
Plant desired nutritional, repairs mine and has preferable recovery dynatron effect.
Embodiment 3:
Iron ore mine, Liaoyang City of Liaoning Province, there is more low-lying land in mine periphery, uses and liquidate without soil tailings method
Ditch and low-lying land Reclamation by filling, comprise the following steps:
(1) Tailing thickening
Concentrating selecting factory new last person ore deposit to send into Paste thickener together with flocculant, flocculant addition is new row
CHARACTERISTICS OF TAILINGS SAND is by by contained dry tailings weight addition per ton bodied ferric sulfate 100g and polyacrylamide 15g.Concentrator overflow
Feeding water return pipeline recycles;
(2) filling low-lying land
The Paste tailings of thickener underflow concentration 70%, for filling low-lying land, comprises the following steps:
Charging stirring: by Paste tailings, slag cements by weight percent: Paste tailings 97%, slag cements 3%, add
Enter agitator stirring 5min.
Consolidation filling: the Paste tailings stirred is delivered to low-lying land heap by belt conveyor and arranges and consolidation.
Leveling: mine tailing is full of after drying up and flattens through bull-dozer.
(3) preparation is without soil mine tailing substrate
Comprise the following steps without soil mine tailing substrate:
Dispensing: according to percetage by weight: iron tailings 40%, turfy soil 40%, Vermiculitum 5%, pumice 4%, Maifanitum 5%,
Decomposed manure 6% is sufficiently mixed uniformly;
Ripening: ripening 8 days of being banked up by the material mixed, during banking up, remains that the moisture of material is
40%~50%.
(4) cover without soil mine tailing substrate
After low-lying land Paste tailings heap row is full of leveling, that is prepared by this mine tailing covers its surface without soil mine tailing substrate
30cm, then carries out vegetation and reclaims.
What the present embodiment was provided has not only processed a large amount of mine tailing without soil tailings method, reduces mine tailing and takes up an area, reduces
Environmental hazard, makes resource of tailings obtain Appropriate application simultaneously, improves resource utilization.There is preferable economic benefit and society's effect
Benefit.Obtained is high without soil mine tailing substrate machine matter content, and water-retaining property and good permeability can improve the physicochemical property of soil, it is provided that
Plant desired nutritional, repairs mine and has preferable recovery dynatron effect.
Claims (4)
1. the method without soil tailings, it is characterised in that comprise the following steps:
(1) Tailing thickening
Concentrating selecting factory's new last person ore in sand form to send into Paste thickener together with flocculant, described new last person's ore in sand form presses dry tail
Sand weight addition per ton described flocculant 95g~130g, the overflow that described concentrator produces is sent into water return pipeline and is recycled;
(2) filling subsidence area, coombe, low-lying land
The Paste tailings of the underflow density 65%~70% that described concentrator produces, filling subsidence area, coombe or low-lying land, then
Leveling;
(3) preparation is without soil mine tailing substrate
Dispensing: according to percetage by weight: mine tailing 30%~40%, turfy soil 40%~50%, Vermiculitum 3%~5%, pumice 3%
~5%, Maifanitum 3%~5%, decomposed manure 6%~10% be sufficiently mixed uniformly;
Ripening: ripening 5-8 days of being banked up by the material mixed, during banking up, remains that the moisture of material is
40%~50%;
(4) cover without soil mine tailing substrate
Described subsidence area, coombe, low-lying land are filled, after leveling, cover its surface, cladding thickness by described without soil mine tailing substrate
For 25-35cm, then carry out vegetation and reclaim.
Method without soil tailings the most according to claim 1, it is characterised in that described flocculant is by bodied ferric sulfate
Form with polyacrylamide, described new last person's ore in sand form by dry tailings weight addition per ton described bodied ferric sulfate 80g~100g and
Described polyacrylamide 15g~30g.
Method without soil tailings the most according to claim 1, it is characterised in that described step (2) subsidence area, punching
Ditch, low-lying land comprise the following steps in reclaiming:
Charging stirring: by described Paste tailings, slag cements by weight percent: Paste tailings 95%~97%, slag cements
3%~5%, add agitator stirring 5min;
Consolidation filling: the stirring thing stirred is delivered to subsidence area, coombe or low-lying land heap row and consolidation;
Leveling: flatten through bull-dozer.
Method without soil tailings the most according to claim 1, it is characterised in that described Vermiculitum granularity is 40 mesh~60
Mesh, described pumice granularity is 60 mesh~80 mesh, and described Maifanitum granularity is 60 mesh~80 mesh.