A kind of environment-friendly type sheepskin garment leather processing technique Download PDFInfo
- Publication number
- CN106222329A CN106222329A CN201610841494.5A CN201610841494A CN106222329A CN 106222329 A CN106222329 A CN 106222329A CN 201610841494 A CN201610841494 A CN 201610841494A CN 106222329 A CN106222329 A CN 106222329A
- Authority
- CN
- China
- Prior art keywords
- leather
- add
- environment
- acid
- sodium
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
nullThe invention discloses a kind of environment-friendly type sheepskin garment leather processing technique,The abnormal smells from the patient produced for clothing leather、Wash durability is poor、Chrome tanning tanning is not environmentally、Produce the defect of bloom,The present invention is with using naringin、N naphthalene 1 base 3 hydroxyl naphthalene 2 Methanamide、Glycine improves the mechanical performance of clothing leather,Sorbitol、2 bromine 2 nitros 1,3 propanol、Pyridoxol、D pantothenylol、Oleamide、Polyacrylamide、2,3 dyhydrobutanedioic acids improve the leather absorption to little molecule acrylic resin,Sorbitol、Mannitol、THPC、Oils and fats and micromolecular compound are fixed by aluminate coupling agent,3 chlorine 2 hydroxypropyl-trimethyl ammonium chlorides、Polymine、Alumen、Titanium dioxide、Pulvis Talci can avoid bloom,And absorb fine molecular compound.
Description
Technical field
The present invention relates to a kind of environment-friendly type clothing leather processing technique, the lowest bloom, the environment-friendly type Corii Caprae seu Ovis of low abnormal smells from the patient
Clothing leather processing technique.
Background technology
Tanning is a step important during rawhide is changed into leather, and the quality of tannery directly influences the thing of finished leather
Physicochemical performance, has important contacting with the value of finished leather.Currently employed main tanning agent is chromic salt, chromic salt
Tanning agent has water-fastness, shelf-stable, has the advantages such as good hydrothermal stability, but the chromium resource in the whole world is limited, and chromium is made
Being a heavy metal species, with the waste liquid produced during its tanning hide, scurf etc. the most inevitably contains trivalent chromium, and these give up containing chromium
Ecological environment will necessarily be damaged by gurry, and the easiest oxidized generation Cr VI of trivalent chromium, therefore
The tanning agent developing a kind of environmental friendliness, tanning effective is present goal in research.Existing chrome-free tanning agent exist price high,
The shortcomings such as tannery is complicated.
Clothing leather requires repeatedly to wash, but at present clothing leather repeatedly washes that to easily cause feel hardening, this be by
Be washed off in micromolecular compound therein, reduce leather hand feeling, simultaneously the least molecule of clothing leather and other
Oils and fats discharges or migrates out Organic substance release, have impact on leather smells and use.
Summary of the invention
The abnormal smells from the patient that produces for clothing leather, wash durability is poor, chrome tanning tanning not environmentally, produce bloom defect,
Invention uses naringin, N-naphthalene-1-base-3-hydroxyl naphthalene-2-Methanamide, glycine to improve the mechanical performance of clothing leather,
Sorbitol, 2-bromo-2-nitro-1,3-propanol, pyridoxol, D-panthenol, oleamide, polyacrylamide, 2,3-dihydroxy fourth two
Acid improves the leather absorption to little molecule acrylic resin, Sorbitol, mannitol, THPC, Aluminate
Oils and fats and micromolecular compound are fixed by coupling agent, 3-chloro-2-hydroxypropyl-trimethyl ammonium chloride, polymine, Alumen,
Titanium dioxide, Pulvis Talci can avoid bloom, and absorb fine molecular compound.
A kind of environment-friendly type sheepskin garment leather processing technique, it is characterised in that:
From the beginning of acid skin scytoblastema, the addition of each operation additive is on the basis of acid tare weight amount:
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 0.8~1.3% sodium formate, 0.3~0.6%
Sodium bicarbonate, 28 DEG C of stirrings 60~90min, sequentially add aluminium tanningagent 3.0~4.2% and substance A 1%, and constantly rotate 1h, it
Rear addition 1.0~1.2% sodium formate regulation pH to 3.5~3.6, stir 50~70min, add the sodium bicarbonate of 1.2~2.0%
Regulation pH to 4.0~5.0, then heats to 30~40 DEG C, stirs 300~400min;
After described tanning step successively carry out drum take horse stand, setting-out get rid of soft, split and shaving deburring step, institute
Stating control leather bilayer thickness in split step is 1.4~1.6cm, then carries out shaving operation, controls the bilayer of described leather
Thickness is 1.2-1.3cm;
(2) retanning: reconcile liquor ratio 150%~200%, add wattle extract 2~3%, little molecule acrylic acid double tanning agent 1~
2%, 40 DEG C rotate 1.5~2h, add 1.1~the retanning modifying agent of 2.2% and leather machine property improver 0.2~
0.6%, rotate 60~70min, add the sodium bicarbonate regulation pH to 4.2~4.5 of 0.2~1.0%, stir 60~80min, use
100% vexed washing 2 times, each 10min;
(3) neutralize, liquor ratio 100%, add sodium formate 1%, 35 DEG C rotate 30min, add sodium bicarbonate 0.4%~
0.6%, 35 DEG C turn 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, add the levelling agent peregal of leather black NG 1%, 1.2~1.5%, 50 DEG C
Rotate 60~90min, add the sulfited fish oil of synthetic fat liquor SE7% and 1.0~2.4%, 50 DEG C rotate 50~
55min, adds oils and fats fixative 0.5% and substance B 0.6%, rotates 30min, adds the first acid for adjusting pH 3.0 of 1.0-2.0%
~4.0, stir 60-70min, go out drum, take horse, be dried according to conventional garment leather technique, get damp again, get rid of soft covering with paint.
Substance A is sodium ethylene diamine tetracetate, 1,2,3,4,5,6-hexamethylene hexacarboxylic acid sodium salts, sodium gluconate, imino group
Any one of disuccinic acid four sodium;Retanning modifying agent be sorbitol, 2-bromo-2-nitro-1,3-propanol, pyridoxol, D-panthenol,
Oleamide, polyacrylamide, 2,3 dihydroxybutanedioic acid any one;Leather machine property improver is naringin, N-
Naphthalene-1-base-3-hydroxyl naphthalene-2-Methanamide, glycine any one;Oils and fats fixative be Sorbitol, mannitol, four
Methylol phosphorus chloride, distearyl acyl-oxygen isopropyl Aluminate any one;Substance B is 3-chloro-2-Hydroxyproyl Trimethyl chlorination
Ammonium, polymine, Alumen, titanium dioxide, talcous any one.
Present invention have an advantage that
(1) naringin, N-naphthalene-1-base-3-hydroxyl naphthalene-2-Methanamide, glycine is used to improve the machinery of clothing leather
Performance.
(2) sorbitol, 2-bromo-2-nitro-1,3-propanol, pyridoxol, D-panthenol, oleamide, polyacrylamide, 2,3-
Dyhydrobutanedioic acid improves the leather absorption to little molecule acrylic resin, reduces haze value.
(3) Sorbitol, mannitol, THPC, aluminate coupling agent (distearyl acyl-oxygen isopropyl aluminic acid
Ester) oils and fats and micromolecular compound are fixed, improve leather water-wash resistance.
(4) 3-chloro-2-hydroxypropyl-trimethyl ammonium chloride, polymine, Alumen, titanium dioxide, Pulvis Talci, butanimide
Micromolecular compound is absorbed, reduces the abnormal flavour of leather, reduce haze value.
(5) raw material Main Ingredients and Appearance used in the present invention is that above-mentioned substance all can reach requirement.
(6) sodium ethylene diamine tetracetate, 1,2,3,4,5,6-hexamethylene hexacarboxylic acid sodium salts, sodium gluconate, imino-diacetic amber
Aluminium tanningagent is fixed by amber acid four sodium, nitrilotriacetic acid, improves the water-wash resistance of aluminium tanningagent.
(7) the pickling liquid of the present invention be liquor ratio be 100%, add the sulphuric acid of 1.0-1.5% and the sodium chloride of 8-13%,
PH is 2.2-2.6, and temperature is 25-28 DEG C, and pickling rotation time is 60-120min, and the operation before pickling is according to conventional garment
Leather technique obtains.
Detailed description of the invention
Example 1
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 0.8% sodium formate, the sodium bicarbonate of 0.3%, 28 DEG C
Stirring 60min, sequentially adds aluminium tanningagent 3.0% and sodium ethylene diamine tetracetate 1%, and constantly rotates 1h, add 1.0% afterwards
Sodium formate regulation pH to 3.5~3.6, stirs 50min, adds the sodium bicarbonate regulation pH to 4.0 of 1.2%, then heats to 30
DEG C, stir 300min;
After described tanning step successively carry out drum take horse stand, setting-out get rid of soft, split and shaving deburring step, institute
Stating control leather bilayer thickness in split step is 1.4cm, then carries out shaving operation, and the bilayer thickness controlling described leather is
1.2cm;
(2) retanning: reconcile liquor ratio 150%, add wattle extract 2%, little molecule acrylic acid double tanning agent 1%, 40 DEG C of rotations
1.5h, adds sorbitol and the naringin 0.2% of 1.1%, rotates 60min, adds the sodium bicarbonate regulation pH to 4.2 of 0.2%,
Stirring 60min, with 100% vexed washing 2 times, each 10min;
(3) neutralize, liquor ratio 100%, addition sodium formate 1%, 35 DEG C of rotation 30min, addition sodium bicarbonate 0.4%, 35 DEG C
Turning 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, adds leather black NG (Henan Chengtai Chemical Technology Co., Ltd.) 1%, 1.2%
Levelling agent peregal, 50 DEG C rotate 60min, add synthetic fat liquor SE's (Shanghai Leather Chemical Plant) 7% and 1.0%
Sulfited fish oil (Dongguan brightness eagle industrial leather company limited), 50 DEG C rotate 50min, add Sorbitol 0.5% and 3-chloro-
2-hydroxypropyl-trimethyl ammonium chloride 0.6%, rotates 30min, adds the first acid for adjusting pH 3.0 of 1.0%, stirs 60min, goes out drum,
Take horse, be dried according to conventional garment leather technique, get damp again, get rid of soft covering with paint.
Example 2
From the beginning of acid skin scytoblastema, the addition of each operation additive is on the basis of acid tare weight amount:
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 1.3% sodium formate, the sodium bicarbonate of 0.6%, 28 DEG C
Stirring 90min, sequentially adds aluminium tanningagent 4.2% and 1,2,3,4,5,6-hexamethylene hexacarboxylic acid sodium salts 1%, and constantly rotates
1h, adds 1.2% sodium formate regulation pH to 3.5~3.6 afterwards, stirs 70min, and the sodium bicarbonate adding 2.0% regulates pH extremely
5.0, then heat to 40 DEG C, stir 400min;
After described tanning step successively carry out drum take horse stand, setting-out get rid of soft, split and shaving deburring step, institute
Stating control leather bilayer thickness in split step is 1.6cm, then carries out shaving operation, and the bilayer thickness controlling described leather is
1.3cm;
(2) retanning: reconcile liquor ratio 200%, add wattle extract 3%, little molecule acrylic acid double tanning agent 2%, 40 DEG C of rotations
2h, adds 2-bromo-2-nitro-1 of 2.2%, 3-propanol and N-naphthalene-1-base-3-hydroxyl naphthalene-2-Methanamide 0.6%, rotates
70min, adds the sodium bicarbonate regulation pH to 4.5 of 1.0%, stirs 80min, with 100% vexed washing 2 times, each 10min;
(3) neutralize, liquor ratio 100%, addition sodium formate 1%, 35 DEG C of rotation 30min, addition sodium bicarbonate 0.6%, 35 DEG C
Turning 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, adds the levelling agent peregal of leather black NG 1%, 1.5%, 50 DEG C of rotations
90min, adds the sulfited fish oil of synthetic fat liquor SE7% and 2.4%, and 50 DEG C rotate 55min, add mannitol
0.5% and polymine 0.6%, rotate 30min, add the formic acid regulation pH4.0 of 2.0%, stir 70min, go out drum, take
Horse, is dried according to conventional garment leather technique, gets damp again, gets rid of soft covering with paint.
Example 3
From the beginning of acid skin scytoblastema, the addition of each operation additive is on the basis of acid tare weight amount:
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 1.0% sodium formate, the sodium bicarbonate of 0.5%, 28 DEG C
Stirring 75min, sequentially adds aluminium tanningagent 3.6% and sodium gluconate 1%, and constantly rotates 1h, add 1.1% formic acid afterwards
Sodium regulation pH to 3.5~3.6, stirs 60min, adds the sodium bicarbonate regulation pH to 4.5 of 1.6%, then heats to 35 DEG C, stir
Mix 350min;
After described tanning step successively carry out drum take horse stand, setting-out get rid of soft, split and shaving deburring step, institute
Stating control leather bilayer thickness in split step is 1.5cm, then carries out shaving operation, and the bilayer thickness controlling described leather is
1.2m;
(2) retanning: reconcile liquor ratio 170%, add wattle extract 2.5%, little molecule acrylic acid double tanning agent 1.5%, 40 DEG C
Rotate 1.5h, add pyridoxol and the glycine 0.4% of 1.6%, rotate 65min, add the sodium bicarbonate regulation pH of 0.6%
To 4.2, stir 70min, with 100% vexed washing 2 times, each 10min;
(3) neutralize, liquor ratio 100%, addition sodium formate 1%, 35 DEG C of rotation 30min, addition sodium bicarbonate 0.5%, 35 DEG C
Turning 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, adds levelling agent peregal (Hai'an, Jiangsu Province of leather black NG 1%, 1.4%
Petrochemical plant), 50 DEG C rotate 75min, add the sulfited fish oil of synthetic fat liquor SE7% and 1.7%, 50 DEG C turn
Dynamic 50min, adds THPC 0.5% and Alumen 0.6%, rotates 30min, adds the first acid for adjusting pH of 1.5%
3.5, stir 65min, go out drum, take horse, be dried according to conventional garment leather technique, get damp again, get rid of soft covering with paint.
Example 4
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 0.8% sodium formate, the sodium bicarbonate of 0.3%, 28 DEG C
Stirring 60min, sequentially adds aluminium tanningagent 3.0% and iminodisuccinic acid four sodium 1%, and constantly rotates 1h, add afterwards
1.0% sodium formate regulation pH to 3.5~3.6, stirs 50min, adds the sodium bicarbonate regulation pH of nitrilotriacetic acid 0.7g and 1.2%
To 4.0, then heat to 30 DEG C, stir 300min;
After described tanning step successively carry out drum take horse stand, setting-out get rid of soft, split and shaving deburring step, institute
Stating control leather bilayer thickness in split step is 1.4cm, then carries out shaving operation, and the bilayer thickness controlling described leather is
1.2cm;
(2) retanning: reconcile liquor ratio 150%, adds wattle extract 2%, little molecule acrylic acid double tanning agent (Xiamen chemistry far for a long time
Company limited) 1%, 40 DEG C rotate 1.5h, add D-panthenol and the glycine 0.2% of 1.1%, rotate 60min, add
The sodium bicarbonate regulation pH to 4.2 of 0.2%, stirs 60min, with 100% vexed washing 2 times, each 10min;
(3) neutralize, liquor ratio 100%, addition sodium formate 1%, 35 DEG C of rotation 30min, addition sodium bicarbonate 0.4%, 35 DEG C
Turning 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, adds leather black NG (Henan Chengtai Chemical Technology Co., Ltd.) 1%, 1.2%
Levelling agent peregal (Jiangsu Hai'an Petrochemical Plant), 50 DEG C rotate 60min, add synthetic fat liquor SE (Shanghai skin
Leather chemical plant) 7% and 1.0% sulfited fish oil (Dongguan brightness eagle industrial leather company limited), 50 DEG C rotate 50min,
Add aluminate coupling agent (distearyl acyl-oxygen isopropyl Aluminate) 0.5%, titanium dioxide 0.6% and butanimide 0.3g, turn
Dynamic 30min, adds the first acid for adjusting pH 3.0 of 1.0%, stirs 60min, goes out drum, take horse, carry out according to conventional garment leather technique
It is dried, gets damp again, gets rid of soft covering with paint.
Using the conventional big front sheepskin garment leather produced and the present invention to carry out contrast experiment, wash conditions is old with reference to [1]
Side forever. the research [J] of Pigskin Water Washable Garment Leather. Chinese leather, 1997, carry out washing and tested for tensile strength, tearing strength, receipts
Contracting temperature and area.
Table 1 wash anteroposterior contraction temperature/DEG C
After washing, the clothing leather of the present invention is not reduced to less than 85 DEG C, and the receipts of the conventional sheepskin garment leather without chrome tanning
Contracting temperature is far below 85 DEG C.
Cross direction tensile strength/MPa before and after table 2 washing
After washing, the clothing leather tensile strength of the present invention reduces little, and the conventional sheepskin garment leather without chrome tanning is anti-
Zhang Qiangdu is greatly reduced.
Looking for 3 process hides engineers to hear the abnormal smells from the patient of the present invention, experiment finds, the abnormal smells from the patient of the present invention substantially to produce less than routine
Sheepskin garment leather, the most respectively at 10 days, 50 days, 180 days observe leather surface situation, find the present invention clothing leather do not have
Bloom produces, and the clothing leather produced greatly has a small amount of bloom to produce.
Table 3 haze value situation
Haze value indirect reaction micromolecular compound therein amount, finds from experiment, the haze value of the present invention is significantly less than
The conventional big clothing leather produced.
Above embodiments of the present invention are explained in detail, but the invention is not restricted to above-mentioned embodiment, in institute
State in the ken that technical field those of ordinary skill is possessed, it is also possible to make on the premise of without departing from present inventive concept
Various amendments.These are all the most creative amendments, as long as all by Patent Law in scope of the presently claimed invention
Protection.
Claims (6)
1. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that:
From the beginning of acid skin scytoblastema, the addition of each operation additive is on the basis of acid tare weight amount:
(1) tanning: surplus 80% liquor ratio in conventional garment leather pickling liquid, adds 0.8~the little Su of 1.3% sodium formate, 0.3~0.6%
Beat, 28 DEG C of stirrings 60~90min, sequentially add aluminium tanningagent 3.0~4.2% and substance A 1%, and constantly rotate 1h, add afterwards
Enter 1.0~1.2% sodium formate regulation pH to 3.5~3.6, stir 50~70min, add 1.2~2.0% sodium bicarbonate regulation
PH to 4.0~5.0, then heats to 30~40 DEG C, stirs 300~400min;
Carry out drum after described tanning step successively and take that horse stands, setting-out gets rid of soft, split and shaving deburring step, described
Controlling leather bilayer thickness in skin step is 1.4~1.6cm, then carries out shaving operation, controls the bilayer thickness of described leather
For 1.2-1.3cm;
(2) retanning: reconcile liquor ratio 150%~200%, add wattle extract 2~3%, little molecule acrylic acid double tanning agent 1~2%,
40 DEG C rotate 1.5~2h, add 1.1~the retanning modifying agent of 2.2% and leather machine property improver 0.2~0.6%, turn
Dynamic 60~70min, add the sodium bicarbonate regulation pH to 4.2~4.5 of 0.2~1.0%, stir 60~80min, with 100% vexed water
Wash 2 times, each 10min;
(3) neutralize, liquor ratio 100%, addition sodium formate 1%, 35 DEG C of rotation 30min, addition sodium bicarbonate 0.4%~0.6%, 35
DEG C turning 40min, pH again is 6.0~6.2, and liquor ratio 100% is washed twice, each 10min, discharge opeing;
(4) dyeing and fat-liquoring: liquor ratio 100%, adds the levelling agent peregal of leather black NG 1%, 1.2~1.5%, 50 DEG C of rotations
60~90min, add the sulfited fish oil of synthetic fat liquor SE7% and 1.0~2.4%, 50 DEG C rotate 50~
55min, adds oils and fats fixative 0.5% and substance B 0.6%, rotates 30min, adds the first acid for adjusting pH 3.0 of 1.0-2.0%
~4.0, stir 60-70min, go out drum, take horse, be dried according to conventional garment leather technique, get damp again, get rid of soft covering with paint.
2. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that: substance A be sodium ethylene diamine tetracetate, 1,2,3,4,
5,6-hexamethylene hexacarboxylic acid sodium salts, sodium gluconate, iminodisuccinic acid four sodium any one.
3. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that: retanning modifying agent be sorbitol, 2-bromo-2-nitro-
1,3-propanol, pyridoxol, D-panthenol, oleamide, polyacrylamide, 2,3 dihydroxybutanedioic acid any one.
4. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that: leather machine property improver is naringin, N-
Naphthalene-1-base-3-hydroxyl naphthalene-2-Methanamide, glycine any one.
5. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that: oils and fats fixative be Sorbitol, mannitol,
THPC, distearyl acyl-oxygen isopropyl Aluminate any one.
6. an environment-friendly type sheepskin garment leather processing technique, it is characterised in that: substance B is 3-chloro-2-Hydroxyproyl Trimethyl chlorination
Ammonium, polymine, Alumen, titanium dioxide, talcous any one.