CN105369619B - 一种兔毛纤维接枝牛奶蛋白改性的工艺 - Google Patents

一种兔毛纤维接枝牛奶蛋白改性的工艺 Download PDF

Info

Publication number
CN105369619B
CN105369619B CN201510793979.7A CN201510793979A CN105369619B CN 105369619 B CN105369619 B CN 105369619B CN 201510793979 A CN201510793979 A CN 201510793979A CN 105369619 B CN105369619 B CN 105369619B
Authority
CN
China
Prior art keywords
milk protein
grafting
bath
rabbit
modified
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201510793979.7A
Other languages
English (en)
Other versions
CN105369619A (zh
Inventor
刘利萍
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tongxiang Jinlong Silk Thread Co., Ltd.
Original Assignee
Huzhou Pin Chuan Brooder Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Huzhou Pin Chuan Brooder Co Ltd filed Critical Huzhou Pin Chuan Brooder Co Ltd
Priority to CN201510793979.7A priority Critical patent/CN105369619B/zh
Publication of CN105369619A publication Critical patent/CN105369619A/zh
Application granted granted Critical
Publication of CN105369619B publication Critical patent/CN105369619B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种新的兔毛纤维接枝牛奶蛋白改性的工艺,其不使用蛋白酶,对纤维无损伤,而且所述工艺天然环保,不使用化学原料,本发明制得的兔毛织物手感更加柔软,细腻,不易起球,还具有特别的光泽度。本发明制得的兔毛织物抗起球等级可以达到4‑5,而且不易掉毛。

Description

一种兔毛纤维接枝牛奶蛋白改性的工艺
技术领域
本发明涉及一种兔毛纤维接枝牛奶蛋白改性的工艺,属于纺织领域。
背景技术
兔毛手感柔软、质轻蓬松、风格别致、保暖性和吸湿性好,但由于兔毛纤维表面存在单向性鳞片,纤维强度低,表面摩擦性能差,卷曲度小,抱合性能差,在纺织品中使用易掉毛、缩水、起毛起球。
树脂型交联剂蔗糖脂肪酸酯缩水甘油醚(SFEGE)对蛋白质接枝一般在中性条件下进行,交联剂是由蔗糖脂肪酸酯与环氧氯丙烷反应生成,其中环氧氯丙烷上的环氧基可以开环与氨基、羟基、硫氢键、羧基、酪氨酸酚羟基结合。在一定的温度条件下,交联剂和蛋白质相连接,通过环氧基将蛋白质连接到兔毛表面,其反应只需氨基、羟基、硫氢键、羧基、酪氨酸酚羟基其中之一即可,即使蛋白质自身交联,也可以将蛋白质接枝到纤维表面,因而纤维表面改性可以直接用交联剂与蛋白质混合进行。
现有技术在进行牛奶蛋白接枝的时候,往往需要用浓硫酸进行预处理才能顺利进行,然而浓硫酸会伤害织物,也不利于环保。
现有技术这些方法在一定程度上解决了兔毛针织物的起毛起球问题,但会损伤纤维,改变织物的风格,限制织物色彩。
本发明旨在提供一种新的兔毛纤维接枝牛奶蛋白改性的工艺,其不需要使用浓酸进行改性,天然环保,不伤织物,而且抗起球效果更好,还能赋予织物更好的防脱性能,力学性能,手感等特质。
发明内容
基于背景技术存在的技术问题,本发明针对背景技术存在的问题,提供一种新的兔毛纤维接枝牛奶蛋白改性的工艺,其不需要使用浓酸进行改性,天然环保,不伤织物,而且抗起球效果更好,还能赋予织物更好的防脱性能,力学性能,手感等特质。
本发明的目的通过以下技术方案实现:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为10-12w/cm,保持恒温40℃处理18-25min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在6~8;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴5-9,min;60℃预烘干22-28min,100℃高温烘焙8-12min,水洗,稍微挤干后在30℃下烘干。
本发明的有益之处在于:
本发明提供一种新的兔毛纤维接枝牛奶蛋白改性的工艺,其不需要使用浓酸进行改性,天然环保,不伤织物,大大缩短时间,尤其是高温处理的时间,减少对织物的伤害,减少对能源的消耗。而且抗起球效果更好,还能赋予织物更好的防脱性能,力学性能,手感等特质。特别是,抗起球等级能达到4-5。
具体实施方式
本发明所用的实验材料:纯兔毛针织物(45tex×2)。
实施例1:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为10w/cm,保持恒温40℃处理25min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在6;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴9,min;60℃预烘干22min,100℃高温烘焙12min,水洗,稍微挤干后在30℃下烘干。
实施例2:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为12w/cm,保持恒温40℃处理18min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在8;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴5,min;60℃预烘干28min,100℃高温烘焙8min,水洗,稍微挤干后在30℃下烘干。
实施例3:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为11w/cm,保持恒温40℃处理24min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在7;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴8,min;60℃预烘干23min,100℃高温烘焙11min,水洗,稍微挤干后在30℃下烘干。
实施例4:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为10w/cm,保持恒温40℃处理19min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在8;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴6,min;60℃预烘干27min,100℃高温烘焙9min,水洗,稍微挤干后在30℃下烘干。
实施例5:
一种新的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为11w/cm,保持恒温40℃处理23min,然后自然风干。
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液:2%的蔗糖脂肪酸酯,2%的牛奶蛋白,2%的平平加O,pH值控制在6;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm,60℃下水浴7,min;60℃预烘干24min,100℃高温烘焙10min,水洗,稍微挤干后在30℃下烘干。
实施例6:
参照标准FZ/T 01046—1996《兔毛产品掉毛量的测定》,采用YG(B)401D型全自动织物平磨仪,模拟织物所处的掉毛环境。
依据GB/T 4802.1-2008《纺织品织物起毛起球性能的测定》中的圆轨迹法、单位面积毛球个数及单位面积毛球称量法的内容进行。
效果测评:
实验结果如下表所示:
表1
此检测数据只针对上述检测样品。
由此可见,本发明提供一种新的兔毛纤维接枝牛奶蛋白改性的方法,其不使用蛋白酶,对纤维无损伤,而且所述工艺天然环保,不使用化学原料,处理后的兔毛织物手感更加柔软,细腻,不易起球,还具有特别的光泽度。
以上所述,仅为本发明较佳的具体实施方式,但本发明的保护范围并不局限于此,任何熟悉本技术领域的技术人员在本发明揭露的技术范围内,根据本发明的技术方案及其发明构思加以等同替换或改变,都应涵盖在本发明的保护范围之内。

Claims (2)

1.一种兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1 g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5 g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为10-12w/cm,保持恒温40℃处理18-25min,然后自然风干;
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液: 2%的蔗糖脂肪酸酯缩水甘油醚,2%的牛奶蛋白,2%的平平加O,pH值控制在6~8;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm, 60℃下水浴5-9min;60℃预烘干22-28min,100℃高温烘焙8-12min,水洗,稍微挤干后在30℃下烘干。
2.权利要求1所述的兔毛纤维接枝牛奶蛋白改性的方法,其步骤如下:
(1)预处理:
配备预处理溶液:纤维素酶0.9g/L,漆酶0.1g/L,蚕丝蛋白1 g/L,鱼皮胶原蛋白0.5g/L,海藻糖0.5 g/L;
预处理工艺为:取兔毛织物水浴浸泡,浴比1:30,放入恒温超声波发生器中,强度为10w/cm,保持恒温40℃处理25min,然后自然风干;
(2)牛奶蛋白接枝处理:
将预处理后的兔毛织物继续进行接枝处理;
配备整理液: 2%的蔗糖脂肪酸酯缩水甘油醚,2%的牛奶蛋白,2%的平平加O,pH值控制在6;
处理工艺为:浴比为1:50,放入恒温超声波发生器中,强度为8w/cm, 60℃下水浴9min;60℃预烘干22min,100℃高温烘焙12min,水洗,稍微挤干后在30℃下烘干。
CN201510793979.7A 2015-11-18 2015-11-18 一种兔毛纤维接枝牛奶蛋白改性的工艺 Active CN105369619B (zh)