CN105328320B - A kind of electric resistance welding method suitable for bus-bar - Google Patents

A kind of electric resistance welding method suitable for bus-bar Download PDF

Info

Publication number
CN105328320B
CN105328320B CN201510877340.7A CN201510877340A CN105328320B CN 105328320 B CN105328320 B CN 105328320B CN 201510877340 A CN201510877340 A CN 201510877340A CN 105328320 B CN105328320 B CN 105328320B
Authority
CN
China
Prior art keywords
bus
bar
lug
welding
contact surface
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201510877340.7A
Other languages
Chinese (zh)
Other versions
CN105328320A (en
Inventor
林雁斌
余万民
周富成
张勇根
狄学锋
张建章
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Zhejiang Haiyue Automation Machinery Co Ltd
Original Assignee
Zhejiang Haiyue Automation Machinery Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Zhejiang Haiyue Automation Machinery Co Ltd filed Critical Zhejiang Haiyue Automation Machinery Co Ltd
Priority to CN201510877340.7A priority Critical patent/CN105328320B/en
Publication of CN105328320A publication Critical patent/CN105328320A/en
Application granted granted Critical
Publication of CN105328320B publication Critical patent/CN105328320B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

A kind of electric resistance welding method suitable for bus-bar, it is related to cell production method field.Resistance heat caused by the contact surface and adjacent domain that this method of the present invention passes through bus-bar and lug using electric current is welded, and the present invention quickly can be welded once to multiple lugs on same bus-bar, improves speed of welding.

Description

A kind of electric resistance welding method suitable for bus-bar
Technical field
The present invention relates to cell production method field, more particularly to a kind of electric resistance welding method suitable for bus-bar.
Background technology
Existing bus-bar welding is main to use two ways, and first way is welded for rifle, and second is melting welding;Wherein A kind of method has not used because environmentally friendly, security problems be present, and second method needs to use 500 DEG C or so of weldering Jointing temp, the huge energy consumption of this method, but efficiency is very low;There is a kind of welding side when welding other objects in the prior art Method is electric resistance welding, and the method for existing resistance welding mainly uses spot welding, and the welding head of electric welding machine be can not be directly to confluxing What the junction of row and lug was welded.
The content of the invention
The present invention provides a kind of electric resistance welding method suitable for bus-bar in view of the deficiencies of the prior art, and this method can Quickly once to be welded to multiple lugs on same bus-bar, speed of welding is improved.
The technical scheme is that providing a kind of electric resistance welding method suitable for bus-bar, this method is passed through using electric current Resistance heat caused by the contact surface and adjacent domain of bus-bar and lug is welded, and is comprised the following steps:
Step 1, the contact surface on the lug with the bus-bar is subjected to solder side forming processes, confluxed described On row with opened up on the contact surface of the lug with the one-to-one welding groove of the lug;
Step 2, by the connection corresponding with the welding groove of the welding ends of described lug;
Step 3, the position of the relatively described lug of the bus-bar is subjected to displacement, is denoted as the first displacement;
Step 4, contact surface and adjacent domain to the bus-bar and the lug carry out energization butt welding or flash welding with Form nugget;
Step 5, power-off forging and stamping, nugget crystallisation by cooling in the case where pressure continues effect is set to form solder joint, forging and stamping distance is denoted as the Two displacements.
As a preference of the present invention, in described step one, the solder side forming processes comprise the following steps:
First step, all lug erecting and welding positions of required welding on a bus-bar are consolidated It is fixed;
Second step, it will carry out being cut to butt welding portion by the welding ends of the fixed lug.
As a preference of the present invention, described butt welding portion is smooth plane.Arrangement sets and can lifted in a planar manner The uniformity in butt welding portion, it is ensured that the success rate once welded.
As a preference of the present invention, the described rectangular dentation in butt welding portion.Butt welding portion is set to protect with the arrangement of rectangular teeth Card during extruding rectangular teeth can fully with busbar contact and eliminate the possibility of rosin joint.
As a preference of the present invention, by the relatively described lug of the bus-bar by way of extruding in described step three Position carry out displacement.
As a preference of the present invention, the first described displacement is 1mm ~ 2mm.
As a preference of the present invention, to the contact surface and proximity of the bus-bar and the lug in described step four Domain carries out energization butt welding.
As a preference of the present invention, to the contact surface and proximity of the bus-bar and the lug in described step four Domain carries out energization flash welding.
As a preference of the present invention, described second displacement is 0.5mm ~ 2mm.
The invention has the advantages that:
The present invention has the advantages of fast and reliable.
Brief description of the drawings
Fig. 1 is the bus-bar of the embodiment of the present invention and the first embodiment of lug;
Fig. 2 is the bus-bar of the embodiment of the present invention and second of embodiment of lug.
In figure:1- bus-bars;2- lugs;3- welding grooves;4- butt welding portion.
Embodiment
The present invention is described in further detail below in conjunction with accompanying drawing.
As shown in Figure 1 to Figure 2, the present embodiment is produced using electric current by the contact surface and adjacent domain of bus-bar 1 and lug 2 Raw resistance heat is welded, and is comprised the following steps:
Step 1, solder side forming processes will be carried out with the contact surface of bus-bar 1 on lug 2, on bus-bar 1 with lug Opened up on 2 contact surface with welding groove 3 one-to-one with lug 2;
Step 2, by the connection corresponding with welding groove 3 of the welding ends of lug 2;
Step 3, position of the bus-bar 1 with respect to lug 2 is subjected to displacement, is denoted as the first displacement;
Step 4, it is molten to be formed that energization butt welding or flash welding are carried out to the contact surface and adjacent domain of bus-bar 1 and lug 2 Core;
Step 5, power-off forging and stamping, nugget crystallisation by cooling in the case where pressure continues effect is set to form solder joint, forging and stamping distance is denoted as the Two displacements.
Position of the bus-bar 1 with respect to lug 2 is subjected to displacement by way of extruding in the present embodiment step 3.First Move as 1mm ~ 2mm.Second displacement is 0.5mm ~ 2mm.
As shown in Figure 1 to Figure 2, in the present embodiment step 1, solder side forming processes comprise the following steps:
First step, the erecting and welding position of all lugs 2 of required welding on a bus-bar 1 is fixed;
Second step, it will carry out being cut to butt welding portion 4 by the welding ends of fixed lug 2.
As shown in figure 1, the first embodiment in the present embodiment butt welding portion 4 is smooth plane.To bus-bar 1 in step 4 Energization butt welding is carried out with the contact surface and adjacent domain of lug 2.
As shown in Fig. 2 second of embodiment in the present embodiment butt welding portion 4 is 4 rectangular dentation of butt welding portion.It is right in step 4 The contact surface and adjacent domain of bus-bar 1 and lug 2 carry out energization flash welding.
Pressing method has two in step 3, and first is that can extrude bus-bar 1 toward the direction of lug 2 in welding, The homogeneous that multiple lugs 2 are carried out by direct-electrifying after once extruding welds, and efficiency is very high;Second be by lug 2 one by one to Bus-bar 1 is extruded, single energization welding after completing extruding, although not as good as first method height of this method efficiency, into Product rate is higher than first method.
Embodiment described above is only that the preferred embodiment of the present invention is described, not to the design of the present invention It is defined with scope.On the premise of design concept of the present invention is not departed from, technical side of the ordinary people in the field to the present invention The all variations and modifications that case is made, all should drop into protection scope of the present invention, the claimed technology contents of the present invention, Through all recording in detail in the claims.

Claims (5)

1. one kind is applied to bus-bar(1)Electric resistance welding method, it is characterised in that this method passes through bus-bar using electric current(1) With lug(2)Contact surface and adjacent domain caused by resistance heat welded, comprise the following steps:
Step 1, by the lug(2)The upper and bus-bar(1)Contact surface carry out solder side forming processes, in the remittance Stream row(1)The upper and lug(2)Contact surface on open up with the lug(2)One-to-one welding groove(3);
Step 2, by described lug(2)Welding ends and the welding groove(3)Corresponding connection;
Step 3, by the bus-bar(1)Relatively described lug(2)Position carry out displacement, be denoted as the first displacement;
Step 4, to the bus-bar(1)With the lug(2)Contact surface and adjacent domain carry out energization butt welding or flash welding To form nugget;
Step 5, power-off forging and stamping, nugget crystallisation by cooling in the case where pressure continues effect is set to form solder joint, forging and stamping distance is denoted as second Move;
In described step one, the solder side forming processes comprise the following steps:
First step, by a bus-bar(1)All lugs of welding needed for upper(2)Erecting and welding position is consolidated It is fixed;
Second step, by by the fixed lug(2)Welding ends carry out being cut to butt welding portion(4);
By the bus-bar by way of extruding in described step three(1)Relatively described lug(2)Position carry out displacement; The first described displacement is 1mm ~ 2mm, and described second displacement is 0.5mm ~ 2mm.
2. one kind according to claim 1 is applied to bus-bar(1)Electric resistance welding method, it is characterised in that:Described pair Weldering portion(4)For smooth plane.
3. one kind according to claim 1 is applied to bus-bar(1)Electric resistance welding method, it is characterised in that:Described pair Weldering portion(4)Rectangular dentation.
4. one kind according to claim 2 is applied to bus-bar(1)Electric resistance welding method, it is characterised in that:Described step To the bus-bar in rapid four(1)With the lug(2)Contact surface and adjacent domain carry out energization butt welding.
5. one kind according to claim 3 is applied to bus-bar(1)Electric resistance welding method, it is characterised in that:Described step To the bus-bar in rapid four(1)With the lug(2)Contact surface and adjacent domain carry out energization flash welding.
CN201510877340.7A 2015-12-04 2015-12-04 A kind of electric resistance welding method suitable for bus-bar Active CN105328320B (en)