CN104594111A - Corrugated paper containing modified ethylene-vinyl acetate copolymer and preparation method of corrugated paper - Google Patents

Corrugated paper containing modified ethylene-vinyl acetate copolymer and preparation method of corrugated paper Download PDF

Info

Publication number
CN104594111A
CN104594111A CN201410844389.8A CN201410844389A CN104594111A CN 104594111 A CN104594111 A CN 104594111A CN 201410844389 A CN201410844389 A CN 201410844389A CN 104594111 A CN104594111 A CN 104594111A
Authority
CN
China
Prior art keywords
vinyl acetate
corrugated paper
polymer
ethene improved
parts
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410844389.8A
Other languages
Chinese (zh)
Inventor
董良清
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HEFEI DANSUN PACKAGING Co Ltd
Original Assignee
HEFEI DANSUN PACKAGING Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HEFEI DANSUN PACKAGING Co Ltd filed Critical HEFEI DANSUN PACKAGING Co Ltd
Priority to CN201410844389.8A priority Critical patent/CN104594111A/en
Publication of CN104594111A publication Critical patent/CN104594111A/en
Pending legal-status Critical Current

Abstract

The invention discloses corrugated paper containing a modified ethylene-vinyl acetate copolymer and a preparation method of the corrugated paper. The corrugated paper containing the modified ethylene-vinyl acetate copolymer comprises the following raw materials in parts by weight: 70 parts of waste paper, 20 parts of the modified ethylene-vinyl acetate copolymer, 10 parts of soybean meal, 2 parts of butadiene styrene rubber, 1 part of lignin fibers, 2 parts of aluminum nitride, 4 parts of a thickening agent and an aluminate coupling agent. The formula is difficultly obtained in the industry, the strength of the corrugated paper produced by virtue of the formula and the process can be greatly improved, and the water resistance of the product can be improved.

Description

A kind of corrugated paper containing ethene improved-vinyl acetate co-polymer and preparation method thereof
Technical field
The present invention relates to a kind of corrugated paper, be specifically related to a kind of corrugated paper containing ethene improved-vinyl acetate co-polymer and preparation method thereof.
Background technology
Corrugated paper is the common materials of paper packaging box, and it has hardness again than wooden case light weight, and size is easily cut out, and is used for other packaged products of protection not to be compromised.Corrugated paper can print pattern and the word of different color or write letter symbol in outside, cost is also relatively cheap.But, corrugated paper avoid water logging, humidity, mouldy, enter water, hand hook etc.But existing corrugated paper is all weak in process of production, intensity and the water proofing property of corrugated paper can not be improved.
Summary of the invention
The object of the present invention is to provide a kind of corrugated paper containing ethene improved-vinyl acetate co-polymer and preparation method thereof.
The present invention adopts following technical scheme:
Corrugated paper containing ethene improved-vinyl acetate co-polymer, is characterized in that the weight portion of its constitutive material is: waste paper 70-80, ethene improved-vinyl acetate co-polymer 20-30, soy meal 10-15, butadiene-styrene rubber 2-4, lignin fibre 1-3, aluminium nitride 2-3, thickener 4-6, aluminate coupling agent 1-1.5, octyl epoxy stearate 2-3, kudzuvine root starch 2-4.
The described corrugated paper containing ethene improved-vinyl acetate co-polymer, is characterized in that the weight portion of its constitutive material is: waste paper 70, ethene improved-vinyl acetate co-polymer 20, soy meal 10, butadiene-styrene rubber 2, lignin fibre 1, aluminium nitride 2, thickener 4, aluminate coupling agent 1, octyl epoxy stearate 2, kudzuvine root starch 2.
The preparation method of the described corrugated paper containing ethene improved-vinyl acetate co-polymer, is characterized in that comprising the following steps:
(1) Waste Paper Handling: obtain paper pulp after fragmentation, making beating, screening, the removal of impurity are carried out to waste paper;
(2) slurrying: put in reactor by the paper pulp handled well, adds ethene improved-vinyl acetate co-polymer, soy meal, butadiene-styrene rubber, lignin fibre, aluminium nitride; Temperature is controlled between 80 DEG C-85 DEG C, stir 3-4 hour continuously;
(3) after step (2) terminates, in reactor, thickener, aluminate coupling agent, octyl epoxy stearate, kudzuvine root starch is added again; Temperature is controlled to stir 1-2 hour at 85-90 DEG C;
(4) terminate rear temperature to be controlled to obtain finished product at 60-75 DEG C in step (3).
Beneficial effect of the present invention:
The present invention's formula is in industry difficult to expect, the corrugated paper intensity produced by its composition and engineering greatly can be improved and can also improve the water resistance of product.
Detailed description of the invention
Embodiment 1: the corrugated paper containing ethene improved-vinyl acetate co-polymer, is characterized in that the weight portion of its constitutive material is: waste paper 70, ethene improved-vinyl acetate co-polymer 20, soy meal 10, butadiene-styrene rubber 2, lignin fibre 1, aluminium nitride 2, thickener 4, aluminate coupling agent 1, octyl epoxy stearate 2, kudzuvine root starch 2.
3, a preparation method for the corrugated paper containing ethene improved-vinyl acetate co-polymer as claimed in claim 1, is characterized in that comprising the following steps:
(1) Waste Paper Handling: obtain paper pulp after fragmentation, making beating, screening, the removal of impurity are carried out to waste paper;
(2) slurrying: put in reactor by the paper pulp handled well, adds ethene improved-vinyl acetate co-polymer, soy meal, butadiene-styrene rubber, lignin fibre, aluminium nitride; Temperature is controlled between 80 DEG C-85 DEG C, stir 3-4 hour continuously;
(3) after step (2) terminates, in reactor, thickener, aluminate coupling agent, octyl epoxy stearate, kudzuvine root starch is added again; Temperature is controlled to stir 1-2 hour at 85-90 DEG C;
(4) terminate rear temperature to be controlled to obtain finished product at 60-75 DEG C in step (3).

Claims (3)

1. the corrugated paper containing ethene improved-vinyl acetate co-polymer, is characterized in that the weight portion of its constitutive material is: waste paper 70-80, ethene improved-vinyl acetate co-polymer 20-30, soy meal 10-15, butadiene-styrene rubber 2-4, lignin fibre 1-3, aluminium nitride 2-3, thickener 4-6, aluminate coupling agent 1-1.5, octyl epoxy stearate 2-3, kudzuvine root starch 2-4.
2. the corrugated paper containing ethene improved-vinyl acetate co-polymer according to claim 1, is characterized in that the weight portion of its constitutive material is: waste paper 70, ethene improved-vinyl acetate co-polymer 20, soy meal 10, butadiene-styrene rubber 2, lignin fibre 1, aluminium nitride 2, thickener 4, aluminate coupling agent 1, octyl epoxy stearate 2, kudzuvine root starch 2.
3. a preparation method for the corrugated paper containing ethene improved-vinyl acetate co-polymer as claimed in claim 1, is characterized in that comprising the following steps:
(1) Waste Paper Handling: obtain paper pulp after fragmentation, making beating, screening, the removal of impurity are carried out to waste paper;
(2) slurrying: put in reactor by the paper pulp handled well, adds ethene improved-vinyl acetate co-polymer, soy meal, butadiene-styrene rubber, lignin fibre, aluminium nitride; Temperature is controlled between 80 DEG C-85 DEG C, stir 3-4 hour continuously;
(3) after step (2) terminates, in reactor, thickener, aluminate coupling agent, octyl epoxy stearate, kudzuvine root starch is added again; Temperature is controlled to stir 1-2 hour at 85-90 DEG C;
(4) terminate rear temperature to be controlled to obtain finished product at 60-75 DEG C in step (3).
CN201410844389.8A 2014-12-25 2014-12-25 Corrugated paper containing modified ethylene-vinyl acetate copolymer and preparation method of corrugated paper Pending CN104594111A (en)