CN104441131A - Method for anticorrosive treatment of willow twigs - Google Patents

Method for anticorrosive treatment of willow twigs Download PDF

Info

Publication number
CN104441131A
CN104441131A CN201410616090.7A CN201410616090A CN104441131A CN 104441131 A CN104441131 A CN 104441131A CN 201410616090 A CN201410616090 A CN 201410616090A CN 104441131 A CN104441131 A CN 104441131A
Authority
CN
China
Prior art keywords
parts
willow
root
wicker
liquid
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410616090.7A
Other languages
Chinese (zh)
Inventor
徐治合
徐艳云
蔡建军
王培龙
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
ANHUI FUNAN COUNTY WANJIAHE CRAFTS Co Ltd
Original Assignee
ANHUI FUNAN COUNTY WANJIAHE CRAFTS Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by ANHUI FUNAN COUNTY WANJIAHE CRAFTS Co Ltd filed Critical ANHUI FUNAN COUNTY WANJIAHE CRAFTS Co Ltd
Priority to CN201410616090.7A priority Critical patent/CN104441131A/en
Publication of CN104441131A publication Critical patent/CN104441131A/en
Pending legal-status Critical Current

Abstract

The invention provides a method for anticorrosive treatment of willow twigs, and relates to the technical field of production of wicker products. The treatment process is performed on live willow twigs on a willow, and the method comprises the following specific steps: (1) injecting an anticorrosive drug solution into the trunk of the willow from a position below a trunk bifurcation of the willow by adopting a transfusion method; (2) determining the initial time for injecting the anticorrosive drug solution into the willow; and (3) determining the cutting time of the willow twigs. The method for anticorrosive treatment of the willow twigs, provided by the invention, is simple in alive tree anticorrosive treatment process, and breaks through the conventional anticorrosive treatment method; after anticorrosive treatment of alive willow twigs, raw woods and plate squared timbers can be directly used outdoors, the economic added value of the willow is promoted, the willow twigs can be directly used for weaving wicker products, the steps for performing anticorrosive treatment on the willow twigs in the conventional willow weaving process are thoroughly changed, the anticorrosive effect is greatly improved, and the utilization ratio of drugs is also greatly promoted compared with that of the conventional method.

Description

A kind of method for anticorrosion treatment of wicker
Technical field
The present invention relates to the production technical field of wicker products, be specifically related to a kind of method for anticorrosion treatment of wicker.
Background technology
Wicker products is the artifacts of China's widespread among the people, " compile basket, compile basket, every household has ".This is because the raw material sources of this technique are very extensive.Basket is compiled in north primary raw material for compiling basket has withy, Chinese tamarisk branch, mulberry shoot, the twigs of the chaste tree, false indigo stem etc. multiple, produces in salt-soda soil and marshland.Wicker products of a great variety, has the polytypes such as seat, basket, basket, dustpan, round-bottomed basket, crate, shallow basket made of wicker or thin bamboo strips, the gaily decorated basket, bamboo strainer, food dish in domestic.Export trade aspect, has formed buck basket, flower pot coat, picnic tableware basket, hanging basket, lampshade, kennel, cat nest, Bird's Nest etc. through developing and design multiple, has formed the appreciation effect that low-grade goods become high-grade, very by the attention of foreign trade department in foreign trade.
The main skill and technique of willow-plaited process has flat sennit, line to compile, strangles volume, builds volume, wrapped edge five kinds.
Wicker products take wicker as primary raw material, but the wicker in use easily infested and mould corruption of generation, cause knitting shortening in service life.Therefore, wicker needs to process before use, uses immersion treatment now more, present inorganic agent many employings chemical agent, and often toxicity is comparatively strong, residual comparatively serious, often causes toxic residue to leak, affect user healthy in knitting use procedure.And prior art is all process felling the wicker got off, the liquid of process is also all adopt the mode of soaking mostly, and the efficiency that liquid enters wicker inside is slow, and also portion is desirable for the effect of mildew-resistant corruption.
Summary of the invention
Technical problem to be solved by this invention is the defect overcoming prior art, proposes further a kind of method for anticorrosion treatment of wicker, and for the treatment of the anticorrosion liquid of wicker.
Technical problem to be solved by this invention realizes by the following technical solutions:
A method for anticorrosion treatment for wicker, is characterized in that, this processing procedure is carried out for the live body wicker on willow, and concrete steps are:
1) below willow trunk crotch, adopt transfusion, in willow trunk, inject anticorrosion liquid;
2) initial time that the anticorrosion liquid of willow injects is determined:
A. the measurement of standing tree leaf flow velocity:
Adopt thermal pulse instrument or observe the flow velocity of trees resin in diel 24 hours with whole tree potometer, within 20 minutes, measure once, analyze the rule of trees flow velocity in 24 hours;
B. according to leaf rule in willow diel, the initial time that anti-corrosion agent injects is determined; When selecting flow velocity the slowest, to living, tree injects anti-corrosion agent, guarantees that anti-corrosion agent has the sufficient time to permeate to radial direction;
C. the duration of anti-corrosion agent injection:
It is 3-4 hour that 1 bottle of 500ml injects the duration, reaches 3-4kg/m to the injection rate to willow live body 3till;
3) wicker fells the determination of time:
After medicament injects timber, the negative pressure produced by tree transpiration effect makes liquid move up with resin, and meanwhile liquid also can carry out horizontal infiltration along the radial direction of trunk; Check whether treetop position exists anticorrosion liquid, when treetop location detection goes out anticorrosion liquid, can fell wicker, stand-by;
Described anti-corrosion agent is the water extraction liquid of Chinese medicine composition, and every kilogram of Chinese medicine composition prepares water extraction liquid 6 kilograms, and described Chinese medicine composition comprises the material component of following weight:
Rosemary 4-8 part, selfheal 5-9 part, red sage root 1-3 part, mother chrysanthemum 2-4 part, dandelion 3-7 part, selfheal 2-4 part, santal 2-6 part, root of Chinese wild ginger 3-7 part, Chinese honey locust 5-9 part, Kadsura Root-bark 3-5 part, cape jasmine 4-8 part, perillaseed 5-9 part, monkshood 2-4 part, felwort 2-4 part, root of langdu 3-7 part, thunder godvine 2-4 part, evodia rutaecarpa 4-8 part, the tuber of dwarf lilyturf 1-3 part, emblic 2-6 part, purslane 3-7 part, gypsum 4-8 part, Ligusticum wallichii 1-3 part, root of Dahurain angelica 2-4 part, moutan bark 3-7 part.
The preferred weight ratio of each raw material of described Chinese medicine composition is: rosemary 6 parts, selfheal 7 parts, the red sage root 2 parts, mother chrysanthemum 3 parts, dandelion 5 parts, selfheal 3 parts, 4 parts, santal, the root of Chinese wild ginger 5 parts, Chinese honey locust 7 parts, Kadsura Root-bark 4 parts, cape jasmine 6 parts, perillaseed 7 parts, monkshood 3 parts, felwort 3 parts, the root of langdu 5 parts, thunder godvine 3 parts, evodia rutaecarpa 6 parts, the tuber of dwarf lilyturf 2 parts, emblic 4 parts, purslane 5 parts, 6 parts, gypsum, Ligusticum wallichii 2 parts, the root of Dahurain angelica 3 parts, moutan bark 5 parts.
For the treatment of an anti-corrosion agent for wicker, be prepared from by the material component of following weight:
Rosemary 4-8 part, selfheal 5-9 part, red sage root 1-3 part, mother chrysanthemum 2-4 part, dandelion 3-7 part, selfheal 2-4 part, santal 2-6 part, root of Chinese wild ginger 3-7 part, Chinese honey locust 5-9 part, Kadsura Root-bark 3-5 part, cape jasmine 4-8 part, perillaseed 5-9 part, monkshood 2-4 part, felwort 2-4 part, root of langdu 3-7 part, thunder godvine 2-4 part, evodia rutaecarpa 4-8 part, the tuber of dwarf lilyturf 1-3 part, emblic 2-6 part, purslane 3-7 part, gypsum 4-8 part, Ligusticum wallichii 1-3 part, root of Dahurain angelica 2-4 part, moutan bark 3-7 part.
The preferred weight ratio preparing each raw material of anti-corrosion agent is: rosemary 6 parts, selfheal 7 parts, the red sage root 2 parts, mother chrysanthemum 3 parts, dandelion 5 parts, selfheal 3 parts, 4 parts, santal, the root of Chinese wild ginger 5 parts, Chinese honey locust 7 parts, Kadsura Root-bark 4 parts, cape jasmine 6 parts, perillaseed 7 parts, monkshood 3 parts, felwort 3 parts, the root of langdu 5 parts, thunder godvine 3 parts, evodia rutaecarpa 6 parts, the tuber of dwarf lilyturf 2 parts, emblic 4 parts, purslane 5 parts, 6 parts, gypsum, Ligusticum wallichii 2 parts, the root of Dahurain angelica 3 parts, moutan bark 5 parts.
A preparation method for wicker anti-corrosion agent, is characterized in that, concrete steps are:
(1) each material component preparing anti-corrosion agent is taken mixture together by weight;
(2) put into container to add water and decoct, first boiled by water with big fire, then young man simmers 20-30min, filter out the dregs of a decoction, taking liquid, amount of water is according to the liquid of the waste after every kilogram of mixture 6 kilograms;
(3) liquid adopts nanofiltration to remove macromolecular substances, i.e. obtained wicker anti-corrosion agent;
Each material component and weight proportion as follows:
Rosemary 4-8 part, selfheal 5-9 part, red sage root 1-3 part, mother chrysanthemum 2-4 part, dandelion 3-7 part, selfheal 2-4 part, santal 2-6 part, root of Chinese wild ginger 3-7 part, Chinese honey locust 5-9 part, Kadsura Root-bark 3-5 part, cape jasmine 4-8 part, perillaseed 5-9 part, monkshood 2-4 part, felwort 2-4 part, root of langdu 3-7 part, thunder godvine 2-4 part, evodia rutaecarpa 4-8 part, the tuber of dwarf lilyturf 1-3 part, emblic 2-6 part, purslane 3-7 part, gypsum 4-8 part, Ligusticum wallichii 1-3 part, root of Dahurain angelica 2-4 part, moutan bark 3-7 part.
Each material component and preferred weight proportion as follows:
Rosemary 6 parts, selfheal 7 parts, the red sage root 2 parts, mother chrysanthemum 3 parts, dandelion 5 parts, selfheal 3 parts, 4 parts, santal, the root of Chinese wild ginger 5 parts, Chinese honey locust 7 parts, Kadsura Root-bark 4 parts, cape jasmine 6 parts, perillaseed 7 parts, monkshood 3 parts, felwort 3 parts, the root of langdu 5 parts, thunder godvine 3 parts, evodia rutaecarpa 6 parts, the tuber of dwarf lilyturf 2 parts, emblic 4 parts, purslane 5 parts, 6 parts, gypsum, Ligusticum wallichii 2 parts, the root of Dahurain angelica 3 parts, moutan bark 5 parts.
Medicament moves and permeates the inspection of uniformity coefficient in trunk:
After wicker is felled, trunk gathers wicker after felling again, studies the infiltration uniformity coefficient of the liquid on different trunk height and radial direction; The wooden color of willow is generally yellow-white, and after ACQ preservative treatment, wooden color, often in light brown, by the change of wood color in trunk, differentiates the uniformity coefficient of medicinal liquid osmosis;
The inspection of wicker antiseptic property.
Beneficial effect of the present invention is:
The invention provides a kind of method for anticorrosion treatment of wicker, tree anticorrosion treatment technology of living is simple, breaches traditional method for anticorrosion treatment; After the preservative treatment of live body willow, log, plate square bar can directly in outdoor applications, also the economic value added of willow is improved, wicker can be directly used in establishment wicker products, revolutionize in traditional willow-plaited process and antiseptic step is carried out to wicker, and antiseptic effect has had large increase, utilization ratio of drug also comparatively conventional method had larger lifting.
Detailed description of the invention
The technological means realized to make the present invention, creation characteristic, reaching object and effect is easy to understand, below in conjunction with specific embodiment, set forth the present invention further, but following embodiment being only the preferred embodiments of the present invention, and not all.Based on the embodiment in embodiment, those skilled in the art under the prerequisite not making creative work obtain other embodiment, all belong to the protection domain of this patent.
Embodiment 1
For the treatment of an anti-corrosion agent for wicker, be prepared from by the material component of following weight:
Rosemary 4g, selfheal 5g, red sage root 1g, mother chrysanthemum 2g, dandelion 3g, selfheal 2g, santal 2g, root of Chinese wild ginger 3g, Chinese honey locust 5g, Kadsura Root-bark 3g, cape jasmine 4g, perillaseed 5g, monkshood 2g, felwort 2g, root of langdu 3g, thunder godvine 2g, evodia rutaecarpa 4g, the tuber of dwarf lilyturf 1g, emblic 2g, purslane 3g, gypsum 4g, Ligusticum wallichii 1g, root of Dahurain angelica 2g, moutan bark 3g.
The preparation method of wicker anti-corrosion agent, is characterized in that, concrete steps are:
(1) each material component preparing anti-corrosion agent is taken mixture together by weight;
(2) put into container to add water and decoct, first boiled by water with big fire, then young man simmers 20-30min, filter out the dregs of a decoction, taking liquid, amount of water is according to the liquid of the waste after every kilogram of mixture 6 kilograms;
(3) liquid adopts nanofiltration to remove macromolecular substances, i.e. obtained wicker anti-corrosion agent.
The method for anticorrosion treatment of wicker, this processing procedure is carried out for the live body wicker on willow, and concrete steps are:
1) below willow trunk crotch, adopt transfusion, in willow trunk, inject anticorrosion liquid;
2) initial time that the anticorrosion liquid of willow injects is determined:
A. the measurement of standing tree leaf flow velocity:
Adopt thermal pulse instrument or observe the flow velocity of trees resin in diel 24 hours with whole tree potometer, within 20 minutes, measure once, analyze the rule of trees flow velocity in 24 hours;
B. according to leaf rule in willow diel, the initial time that anti-corrosion agent injects is determined; When selecting flow velocity the slowest, to living, tree injects anti-corrosion agent, guarantees that anti-corrosion agent has the sufficient time to permeate to radial direction;
C. the duration of anti-corrosion agent injection:
It is 3-4 hour that every bottle of 500ml injects the duration, reaches 3-4kg/m to the injection rate to willow live body 3till;
3) wicker fells the determination of time:
After medicament injects timber, the negative pressure produced by tree transpiration effect makes liquid move up with resin, and meanwhile liquid also can carry out horizontal infiltration along the radial direction of trunk; Check whether treetop position exists anticorrosion liquid, when treetop location detection goes out anticorrosion liquid, can fell wicker, stand-by.
Embodiment 2
For the treatment of an anti-corrosion agent for wicker, be prepared from by the material component of following weight:
Rosemary 8g, selfheal 9g, red sage root 3g, mother chrysanthemum 4g, dandelion 7g, selfheal 4g, santal 6g, root of Chinese wild ginger 7g, Chinese honey locust 9g, Kadsura Root-bark 5g, cape jasmine 8g, perillaseed 9g, monkshood 4g, felwort 4g, root of langdu 7g, thunder godvine 4g, evodia rutaecarpa 8g, the tuber of dwarf lilyturf 3g, emblic 6g, purslane 7g, gypsum 8g, Ligusticum wallichii 3g, root of Dahurain angelica 4g, moutan bark 7g.
The preparation method of wicker anti-corrosion agent, is characterized in that, concrete steps are:
(1) each material component preparing anti-corrosion agent is taken mixture together by weight;
(2) put into container to add water and decoct, first boiled by water with big fire, then young man simmers 20-30min, filter out the dregs of a decoction, taking liquid, amount of water is according to the liquid of the waste after every kilogram of mixture 6 kilograms;
(3) liquid adopts nanofiltration to remove macromolecular substances, i.e. obtained wicker anti-corrosion agent.
The method for anticorrosion treatment of wicker, this processing procedure is carried out for the live body wicker on willow, and concrete steps are:
1) below willow trunk crotch, adopt transfusion, in willow trunk, inject anticorrosion liquid;
2) initial time that the anticorrosion liquid of willow injects is determined:
A. the measurement of standing tree leaf flow velocity:
Adopt thermal pulse instrument or observe the flow velocity of trees resin in diel 24 hours with whole tree potometer, within 20 minutes, measure once, analyze the rule of trees flow velocity in 24 hours;
B. according to leaf rule in willow diel, the initial time that anti-corrosion agent injects is determined; When selecting flow velocity the slowest, to living, tree injects anti-corrosion agent, guarantees that anti-corrosion agent has the sufficient time to permeate to radial direction;
C. the duration of anti-corrosion agent injection:
It is 3-4 hour that every bottle of 500ml injects the duration, reaches 3-4kg/m to the injection rate to willow live body 3till;
3) wicker fells the determination of time:
After medicament injects timber, the negative pressure produced by tree transpiration effect makes liquid move up with resin, and meanwhile liquid also can carry out horizontal infiltration along the radial direction of trunk; Check whether treetop position exists anticorrosion liquid, when treetop location detection goes out anticorrosion liquid, can fell wicker, stand-by.
Embodiment 3
For the treatment of an anti-corrosion agent for wicker, be prepared from by the material component of following weight:
Rosemary 6g, selfheal 7g, red sage root 2g, mother chrysanthemum 3g, dandelion 5g, selfheal 3g, santal 4g, root of Chinese wild ginger 5g, Chinese honey locust 7g, Kadsura Root-bark 4g, cape jasmine 6g, perillaseed 7g, monkshood 3g, felwort 3g, root of langdu 5g, thunder godvine 3g, evodia rutaecarpa 6g, the tuber of dwarf lilyturf 2g, emblic 4g, purslane 5g, gypsum 6g, Ligusticum wallichii 2g, root of Dahurain angelica 3g, moutan bark 5g.
The preparation method of wicker anti-corrosion agent, is characterized in that, concrete steps are:
(1) each material component preparing anti-corrosion agent is taken mixture together by weight;
(2) put into container to add water and decoct, first boiled by water with big fire, then young man simmers 20-30min, filter out the dregs of a decoction, taking liquid, amount of water is according to the liquid of the waste after every kilogram of mixture 6 kilograms;
(3) liquid adopts nanofiltration to remove macromolecular substances, i.e. obtained wicker anti-corrosion agent.
The method for anticorrosion treatment of wicker, this processing procedure is carried out for the live body wicker on willow, and concrete steps are:
1) below willow trunk crotch, adopt transfusion, in willow trunk, inject anticorrosion liquid;
2) initial time that the anticorrosion liquid of willow injects is determined:
A. the measurement of standing tree leaf flow velocity:
Adopt thermal pulse instrument or observe the flow velocity of trees resin in diel 24 hours with whole tree potometer, within 20 minutes, measure once, analyze the rule of trees flow velocity in 24 hours;
B. according to leaf rule in willow diel, the initial time that anti-corrosion agent injects is determined; When selecting flow velocity the slowest, to living, tree injects anti-corrosion agent, guarantees that anti-corrosion agent has the sufficient time to permeate to radial direction;
C. the duration of anti-corrosion agent injection:
It is 3-4 hour that every bottle of 500ml injects the duration, reaches 3-4kg/m to the injection rate to willow live body 3till;
3) wicker fells the determination of time:
After medicament injects timber, the negative pressure produced by tree transpiration effect makes liquid move up with resin, and meanwhile liquid also can carry out horizontal infiltration along the radial direction of trunk; Check whether treetop position exists anticorrosion liquid, when treetop location detection goes out anticorrosion liquid, can fell wicker, stand-by.
More than show and describe general principle of the present invention, principal character and advantage of the present invention.The technical staff of the industry should understand; the present invention is not restricted to the described embodiments; what describe in above-described embodiment and description is only preference of the present invention; be not used for limiting the present invention; without departing from the spirit and scope of the present invention; the present invention also has various changes and modifications, and these changes and improvements all fall in the claimed scope of the invention.Application claims protection domain is defined by appending claims and equivalent thereof.

Claims (2)

1. a method for anticorrosion treatment for wicker, is characterized in that, this processing procedure is carried out for the live body wicker on willow, and concrete steps are:
1) below willow trunk crotch, adopt transfusion, in willow trunk, inject anticorrosion liquid;
2) initial time that the anticorrosion liquid of willow injects is determined:
A. the measurement of standing tree leaf flow velocity:
Adopt thermal pulse instrument or observe the flow velocity of trees resin in diel 24 hours with whole tree potometer, within 20 minutes, measure once, analyze the rule of trees flow velocity in 24 hours;
B. according to leaf rule in willow diel, the initial time that anti-corrosion agent injects is determined; When selecting flow velocity the slowest, to living, tree injects anti-corrosion agent, guarantees that anti-corrosion agent has the sufficient time to permeate to radial direction;
C. the duration of anti-corrosion agent injection:
It is 3-4 hour that 1 bottle of 500ml injects the duration, reaches 3-4kg/m to the injection rate to willow live body 3till;
3) wicker fells the determination of time:
After medicament injects timber, the negative pressure produced by tree transpiration effect makes liquid move up with resin, and meanwhile liquid also can carry out horizontal infiltration along the radial direction of trunk; Check whether treetop position exists anticorrosion liquid, when treetop location detection goes out anticorrosion liquid, can fell wicker, stand-by;
Described anti-corrosion agent is the water extraction liquid of Chinese medicine composition, and every kilogram of Chinese medicine composition prepares water extraction liquid 6 kilograms, and described Chinese medicine composition comprises the material component of following weight:
Rosemary 4-8 part, selfheal 5-9 part, red sage root 1-3 part, mother chrysanthemum 2-4 part, dandelion 3-7 part, selfheal 2-4 part, santal 2-6 part, root of Chinese wild ginger 3-7 part, Chinese honey locust 5-9 part, Kadsura Root-bark 3-5 part, cape jasmine 4-8 part, perillaseed 5-9 part, monkshood 2-4 part, felwort 2-4 part, root of langdu 3-7 part, thunder godvine 2-4 part, evodia rutaecarpa 4-8 part, the tuber of dwarf lilyturf 1-3 part, emblic 2-6 part, purslane 3-7 part, gypsum 4-8 part, Ligusticum wallichii 1-3 part, root of Dahurain angelica 2-4 part, moutan bark 3-7 part.
2. the method for anticorrosion treatment of wicker according to claim 1, is characterized in that: the preferred weight ratio of each raw material of described Chinese medicine composition is: rosemary 6 parts, selfheal 7 parts, the red sage root 2 parts, mother chrysanthemum 3 parts, dandelion 5 parts, selfheal 3 parts, 4 parts, santal, the root of Chinese wild ginger 5 parts, Chinese honey locust 7 parts, Kadsura Root-bark 4 parts, cape jasmine 6 parts, perillaseed 7 parts, monkshood 3 parts, felwort 3 parts, the root of langdu 5 parts, thunder godvine 3 parts, evodia rutaecarpa 6 parts, the tuber of dwarf lilyturf 2 parts, emblic 4 parts, purslane 5 parts, 6 parts, gypsum, Ligusticum wallichii 2 parts, the root of Dahurain angelica 3 parts, moutan bark 5 parts.
CN201410616090.7A 2014-11-04 2014-11-04 Method for anticorrosive treatment of willow twigs Pending CN104441131A (en)