CN104415898A - Painting method of all-wood door and window - Google Patents

Painting method of all-wood door and window Download PDF

Info

Publication number
CN104415898A
CN104415898A CN201310388321.9A CN201310388321A CN104415898A CN 104415898 A CN104415898 A CN 104415898A CN 201310388321 A CN201310388321 A CN 201310388321A CN 104415898 A CN104415898 A CN 104415898A
Authority
CN
China
Prior art keywords
window
solid wood
wood door
mopping
polishing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201310388321.9A
Other languages
Chinese (zh)
Inventor
吴国权
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HUZHOU NANXUN XIANGLONG WOOD FACTORY
Original Assignee
HUZHOU NANXUN XIANGLONG WOOD FACTORY
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HUZHOU NANXUN XIANGLONG WOOD FACTORY filed Critical HUZHOU NANXUN XIANGLONG WOOD FACTORY
Priority to CN201310388321.9A priority Critical patent/CN104415898A/en
Publication of CN104415898A publication Critical patent/CN104415898A/en
Pending legal-status Critical Current

Abstract

The invention discloses a painting method of all-wood door and window, wherein the painting method comprises the following steps: polishing the surfaces of the all-wood door and window which are coated with the bottom color, polishing and cleaning the dust and the dirty marks on the surfaces, then painting a varnish for several times, drying and polishing, thus making the surfaces of the all-wood door and window beautiful and elegant. The purpose of the invention is to provide a painting method of all-wood door and window; the method is able to solve the problems that the paint film curls, cracks, breaks into small pieces and falls off, and the flow fall problems that the paint film after painting flows downwards, forms beads, drop curtain, and the like, and the problem that wrinkle is formed after the paint film is dried, as well as the problem that bubble or brush texture is formed on the surfaces of the painted door and window; moreover, the method can further solve the problems that the door and window are deformed or even corrupted after being exposed to wind and rain for a long time.

Description

A kind of mopping method of solid wood door and window
Technical field
The present invention relates to a kind of mopping method of solid wood door and window, belong to woodwork manufacture field.
Background technology
Door and window is the requisite part in house, by door and window can with outside world exchange and conmmunication, simultaneously door and window brings sunlight and warm to us, resists extraneous wind and rain and noise.Solid wood door and window with simple and unsophisticated, environmental protection, elegant and poised for feature, dark liking by common people.The outward appearance of door and window also embodies the taste of one way of life.In order to protect wooden door and window and make wooden doors and windows's outward appearance beautiful, usually adopt the mode of mopping to door and window decoration and protection.Often there is a lot of problem in mopping, such as: 1, have paint film to roll, ftracture, be broken into small pieces after come off; 2, after mopping, oil film trickles downwards, forms the stream such as teardrop, canopy pendant problem; 3, fold and problem of non-uniform can be formed after drying varniss; 4, the door and window surface of swiped through paint forms bubble or brush line problem etc., and these problems make the image appearance of door and window be badly damaged, and makes door and window distortion even make door and window rot through long-term exposing to wind and rain.
Summary of the invention
The object of the present invention is to provide a kind of mopping method of solid wood door and window, by the method can solve paint film roll, ftracture, be broken into small pieces after after the problem that comes off and mopping oil film trickle downwards, form the problem of the stream such as teardrop, canopy pendant, and the door and window surface that can form fold and uneven problem and swiped through paint after drying varniss forms the problem of bubble or brush line, in addition, can also solve through long-term exposing to wind and rain make door and window be out of shape even make door and window rot etc. problem.
Technical scheme of the present invention:
A mopping method for solid wood door and window, comprises the steps:
Step a, Base coating: carry out Base coating to solid wood door and window by spraying equipment, carries out coloring grounding to wooden door and window, makes solid wood door and window have certain color;
Step b, once polishes: use cloth to wipe with and wash polishing solid wood door and window surface, and solid wood door and window is reached can the technological requirement of mopping, and make varnish be attached to solid wood door and window surface more securely, the problem avoiding paint film to roll occurs;
Step c, a mopping: after getting varnish dilution, dip varnish with brush and mopping process is carried out to solid wood door and window;
Steps d, dries: dried in the place that the solid wood door and window after mopping is placed on ventilation, notes keeping the drying of environment with clean simultaneously;
Step e, secondary is polished: after door and window dries by the time, then polish to solid wood door and window surface, after varnish parches, use fine sandpaper that furniture is polished one time from the beginning to the end again, this time polishing is to the uneven place that varnish is brushed is polished flat, continue mopping after being beneficial to.
Step f, secondary mopping: after secondary polishing, with brush brush second paint again, during second time mopping, varnish need not dilute, because varnish is denseer, when dipping varnish, the varnish once dipped is unsuitable too many, it is suitable that varnish brush soaks into varnish, and meanwhile, the amount at every turn dipping varnish should keep identical, ensure do not occur that oil film trickles downwards, formed teardrop, canopy etc. stream pendant problem and formed bubble and and particle problem occur;
Step g, dries: the solid wood door and window through secondary mopping dries again, identical with the method for operating of steps d again;
Step h, three polishings: third time polishing is carried out to the solid wood door and window surface of again drying, identical with the method for operating of step e;
Step I, three moppings: the solid wood door and window after third time polishing carries out third time mopping again, identical with the method for operating of step f;
Step j, dries: dried by the solid wood door and window of third time mopping again, identical with the method for operating of steps d;
Step k, cleans polishing: with cloth, solid wood door and window lacquer painting is carried out scouring polishing.
According to the mopping method of aforesaid a kind of solid wood door and window, step c selects varnish, by adding gasoline or transparent glue dilutes varnish, adds gasoline or 25% ~ 40% glue of 20% ~ 30% in the varnish just opened.
According to the mopping method of aforesaid a kind of solid wood door and window, the scrubbing polishing method of step b uses cloth or fine sandpaper to carry out wiping or polishing to solid wood door and window surface, makes solid wood door and window surface color homogeneous phase same, ensure without holiday, colourless grain.
According to the mopping method of aforesaid a kind of solid wood door and window, the mopping method of step c, step f and step I, according to from top to bottom, mopping method from left to right carries out mopping, carry out mopping along wood grain simultaneously, ensure not leak brush, repeatedly staggered mopping method should not be adopted, avoid door and window surface to form bubble or brush line.
According to the mopping method of aforesaid a kind of solid wood door and window, the polishing process of step e and step h, first carries out mild abrasion with No. 0 sand paper by solid wood door and window surface, is not revealed by face side, re-uses cloth and polishing is carried out on solid wood door and window surface.
According to the mopping method of aforesaid a kind of solid wood door and window, steps d, step g and step j dry in step, and place solid wood door and window being placed on drying and free from dust carries out drying process.
According to the mopping method of aforesaid a kind of solid wood door and window, steps d, step g and step j dry in step, and temperature is under the environment of 15 degree ~ 40 degree, and the temperature difference is no more than 15 degree.
According to the mopping method of aforesaid a kind of solid wood door and window, step e, step f and step g carry out 3 ~ 10 times in order, can determine concrete number of operations according to the environment for use of solid wood door and window.
Compared with prior art, this invention is a kind of mopping method providing solid wood door and window, by the method can solve paint film roll, ftracture, be broken into small pieces after after the problem that comes off and mopping oil film trickle downwards, form the problem of the stream such as teardrop, canopy pendant, and the door and window surface of the problem and swiped through paint that can form fold after drying varniss forms the problem of bubble or brush line, in addition, can also solve through long-term exposing to wind and rain make door and window be out of shape even make door and window rot etc. problem.
Detailed description of the invention
Implementation method 1 of the present invention: a kind of mopping method of solid wood door and window, comprises the steps:
Step a, Base coating: choose suitable background color, carries out Base coating by spraying equipment to solid wood door and window;
Step b, once polish: use cloth to wipe with and wash polishing solid wood door and window surface, scrubbing polishing method uses cloth or fine sandpaper to carry out wiping or polishing to solid wood door and window surface, makes solid wood door and window surface color homogeneous phase same, ensure without holiday, colourless grain;
Step c, a mopping: first select the good varnish of quality, the gasoline adding 20% ~ 30% in the varnish just opened dilutes varnish, dips varnish with brush and carries out mopping process to solid wood door and window; Select the varnish that dense rare degree is suitable, when varnish is denseer, add suitable gasoline or transparent glue, according to from top to bottom, mopping method from left to right carries out mopping, carries out mopping along wood grain simultaneously, ensures not leak brush.
Steps d, dries: place solid wood door and window being placed on drying and free from dust carries out drying process;
Step e, secondary is polished: after door and window dries by the time, suitably polished in solid wood door and window surface again, first with No. 0 sand paper, mild abrasion is carried out on solid wood door and window surface, face side is not revealed, re-use cloth and polishing is carried out on solid wood door and window surface, this time polishing is to the uneven place that varnish is brushed is polished flat, continue mopping after being beneficial to;
Step f, secondary mopping: after secondary polishing, with brush brush second paint again.During second time mopping, varnish need not dilute, because varnish is denseer, when dipping varnish, the varnish once dipped is unsuitable too many, and it is suitable that varnish brush soaks into varnish, simultaneously, the amount at every turn dipping varnish should keep identical, according to from top to bottom, mopping method from left to right carries out mopping, carries out mopping along wood grain simultaneously, ensure not leak brush, repeatedly staggered mopping method should not be adopted.Ensure do not occur that oil film trickles downwards, formed teardrop, canopy etc. stream pendant, formed bubble and and particle problem occur;
Step g, dries: the solid wood door and window through secondary mopping dries again, identical with the method for operating of steps d again;
Step h, three polishings: third time polishing is carried out to the solid wood door and window surface of again drying, identical with the method for operating of step e;
Step I, three moppings: the solid wood door and window after third time polishing carries out third time mopping again, identical with the method for operating of step f;
Step j, dries: dried by the solid wood door and window of third time mopping again, identical with the method for operating of steps d;
Step k, cleans polishing: with cloth, solid wood door and window lacquer painting is carried out scouring polishing.
Steps d, step g and step j dry in step, and temperature is dried under the environment of 15 degree ~ 25 degree.
Wherein step e, step f and step g carry out 3 operations in order.
Implementation method 2 of the present invention: a kind of mopping method of solid wood door and window, comprises the steps:
Step a, Base coating: choose suitable background color, carries out Base coating by spraying equipment to solid wood door and window;
Step b, once polish: use cloth to wipe with and wash polishing solid wood door and window surface, scrubbing polishing method uses cloth or fine sandpaper to carry out wiping or polishing to solid wood door and window surface, makes solid wood door and window surface color homogeneous phase same, ensure without holiday, colourless grain;
Step c, a mopping: first select the good varnish of quality, the gasoline adding 20% ~ 30% in the varnish just opened dilutes varnish, dips varnish with brush and carries out mopping process to solid wood door and window, select the varnish that dense rare degree is suitable, when varnish is denseer, add suitable gasoline or transparent glue, according to from top to bottom, mopping method from left to right carries out mopping, carry out mopping along wood grain simultaneously, ensure not leak brush, staggered, firmly to rub brush mopping method should not be adopted repeatedly.
Steps d, dries: solid wood door and window is placed on drying, the place of ventilation and free from dust carries out drying process;
Step e, secondary is polished: after door dries by the time, suitably polished in solid wood door and window surface again, first with No. 0 sand paper, mild abrasion is carried out on solid wood door and window surface, face side is not revealed, re-use cloth and polishing is carried out on solid wood door and window surface, this time polishing is to the uneven place that varnish is brushed is polished flat, continue mopping after being beneficial to;
Step f, secondary mopping: after secondary polishing, with brush brush second paint again.During second time mopping, varnish need not dilute, because varnish is denseer, when dipping varnish, the varnish once dipped is unsuitable too many, and it is suitable that varnish brush soaks into varnish, simultaneously, the amount at every turn dipping varnish should keep identical, according to from top to bottom, mopping method from left to right carries out mopping, carries out mopping along wood grain simultaneously, ensure not leak brush, repeatedly staggered mopping method should not be adopted.Ensure do not occur that oil film trickles downwards, formed teardrop, canopy etc. stream pendant, formed bubble and and particle problem occur;
Step g, dries: the solid wood door and window through secondary mopping dries again, identical with the method for operating of steps d again;
Step h, three polishings: third time polishing is carried out to the solid wood door and window surface of again drying, identical with the method for operating of step e;
Step I, three moppings: the solid wood door and window after third time polishing carries out third time mopping again, identical with the method for operating of step f;
Step j, dries: dried by the solid wood door and window of third time mopping again, identical with the method for operating of steps d;
Step k, cleans polishing: with cloth, solid wood door and window lacquer painting is carried out scouring polishing.
Steps d, step g and step j dry in step, and temperature is dried under the environment of 25 degree ~ 35 degree.
Wherein step e, step f and step g carry out 10 operations in order.
Implementation method 3 of the present invention: a kind of mopping method of solid wood door and window, comprises the steps:
Step a, Base coating: choose suitable background color, carries out Base coating by spraying equipment to solid wood door and window;
Step b, once polish: use cloth to wipe with and wash polishing solid wood door and window surface, scrubbing polishing method uses cloth or fine sandpaper to carry out wiping or polishing to solid wood door and window surface, makes solid wood door and window surface color homogeneous phase same, ensure without holiday, colourless grain;
Step c, a mopping: first select the good varnish of quality, adds 25% ~ 40% glue and dilutes varnish in the varnish just opened, and dips varnish carry out mopping process to solid wood door and window with brush, select the varnish that dense rare degree is suitable, when varnish is denseer, add suitable gasoline or transparent glue, according to from top to bottom, mopping method from left to right carries out mopping, carry out mopping along wood grain simultaneously, ensure not leak brush, staggered, firmly to rub brush mopping method should not be adopted repeatedly.
Steps d, dries: solid wood door and window is placed on drying, the place of ventilation and free from dust carries out drying process;
Step e, secondary is polished: after door dries by the time, suitably polished in solid wood door and window surface again, first with No. 0 sand paper, mild abrasion is carried out on solid wood door and window surface, face side is not revealed, re-use cloth and polishing is carried out on solid wood door and window surface, this time polishing is to the uneven place that varnish is brushed is polished flat, continue mopping after being beneficial to;
Step f, secondary mopping: after secondary polishing, with brush brush second paint again.During second time mopping, varnish need not dilute, because varnish is denseer, when dipping varnish, the varnish once dipped is unsuitable too many, and it is suitable that varnish brush soaks into varnish, simultaneously, the amount at every turn dipping varnish should keep identical, according to from top to bottom, mopping method from left to right carries out mopping, carries out mopping along wood grain simultaneously, ensure not leak brush, repeatedly staggered mopping method should not be adopted.Ensure do not occur that oil film trickles downwards, formed teardrop, canopy etc. stream pendant, formed bubble and and particle problem occur;
Step g, dries: the solid wood door and window through secondary mopping dries again, identical with the method for operating of steps d again;
Step h, three polishings: third time polishing is carried out to the solid wood door and window surface of again drying, identical with the method for operating of step e;
Step I, three moppings: the solid wood door and window after third time polishing carries out third time mopping again, identical with the method for operating of step f;
Step j, dries: dried by the solid wood door and window of third time mopping again, identical with the method for operating of steps d;
Step k, cleans polishing: with cloth, solid wood door and window lacquer painting is carried out scouring polishing.
Steps d, step g and step j dry in step, and temperature is dried under the environment of 30 degree ~ 40 degree.
Wherein step e, step f and step g carry out 5 operations in order.

Claims (8)

1. a mopping method for solid wood door and window, its feature comprises the steps:
Step a, Base coating: Base coating is carried out to solid wood door and window by spraying equipment;
Step b, once polishes: use cloth to wipe with and wash polishing solid wood door and window surface;
Step c, a mopping: after getting varnish dilution, dip varnish with brush and mopping process is carried out to solid wood door and window;
Steps d, dries: dried in the place that the solid wood door and window after mopping is placed on ventilation;
Step e, secondary is polished: after door and window dries by the time, then polish to solid wood door and window surface;
Step f, secondary mopping: after secondary polishing, with brush brush second paint again;
Step g, dries: the solid wood door and window through secondary mopping dries again again;
Step h, three polishings: third time polishing is carried out to the solid wood door and window surface of again drying;
Step I, three moppings: the solid wood door and window after third time polishing carries out third time mopping again;
Step j, dries: dried by the solid wood door and window of third time mopping again;
Step k, cleans polishing: with cloth, solid wood door and window lacquer painting is carried out scouring polishing.
2. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: step c selects varnish, by adding gasoline or transparent glue dilutes varnish.
3. the mopping method of a kind of solid wood door and window according to claim 1, it is characterized in that: a polishing process of step b uses cloth or fine sandpaper to carry out wiping or polishing to solid wood door and window surface, make solid wood door and window surface color homogeneous phase same, ensure without holiday, colourless grain.
4. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: the mopping method of step c, step f and step I, and according to from top to bottom, mopping method from left to right carries out mopping, carries out mopping along wood grain simultaneously.
5. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: the polishing process of step e and step h, first with No. 0 sand paper, mild abrasion is carried out on solid wood door and window surface, re-uses cloth and polishing is carried out on solid wood door and window surface.
6. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: steps d, step g and step j dry in step, is that place solid wood door and window being placed on drying and free from dust carries out drying process.
7. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: steps d, step g and step j dry in step, is to dry under temperature 15 degree ~ 40 degree temperature difference are no more than 15 degree of environment.
8. the mopping method of a kind of solid wood door and window according to claim 1, is characterized in that: step e, step f and step g repeat 3 ~ 10 times in order.
CN201310388321.9A 2013-08-30 2013-08-30 Painting method of all-wood door and window Pending CN104415898A (en)