CN103643437A - Finishing technology for textile fabric - Google Patents
Finishing technology for textile fabric Download PDFInfo
- Publication number
- CN103643437A CN103643437A CN201310604780.6A CN201310604780A CN103643437A CN 103643437 A CN103643437 A CN 103643437A CN 201310604780 A CN201310604780 A CN 201310604780A CN 103643437 A CN103643437 A CN 103643437A
- Authority
- CN
- China
- Prior art keywords
- face fabric
- weaving face
- textile fabric
- tentering
- machine
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
A disclosed finishing technology for textile fabric comprises the following steps: performing singeing on the front surface and the back surface of the textile fabric by a singeing machine with a speed of 150 m/min, wherein the flame temperature during singeing is 1250-1300 DEG C and the singeing grade is sixth grade; immersing the textile fabric with amylase, pushing the textile fabric in a slack manner to a desizing machine, steaming at 120-125 DEG C for 35-40 min, wherein the desizing rate is 97%; performing three-time water washing and two-time washing on the front surface and the back surface of the textile fabric, wherein the water washing temperature is 70 DEG C and the water washing time is 30-35 min; drying by a roller with a temperature of 80 DEG C, then drying by a roller with a temperature of 160 DEG C; putting the dried textile fabric in a needle-plate tentering machine for tentering, wherein the humidity in the tentering machine is 8%; performing preshrinking on the tentered textile fabric; and performing ironing shape-setting at 120-125 DEG C for 20-25 min. The finishing technology provided by the invention belongs to a purely physical finishing technology, no chemical preparations are needed and the pollution is reduced.
Description
Technical field
The present invention relates to the finishing technique of weaving face fabric.
Background technology
A large amount of each analog assistants that use of rear arrangement stage of fabric production, to fabric and the unbearable severity of environmental pollution, and make the activation composition of many natural materials be killed in addition, and dress or use are all undesirable with the service life that extends clothes to playing skin care.
Summary of the invention
The object of the present invention is to provide a kind of finishing technique of weaving face fabric, it has adopted pure physical finishing technique, without using chemicals, has reduced pollution.
For achieving the above object, technical scheme of the present invention is the finishing technique of a kind of weaving face fabric of design, comprises the steps:
Adopt the gassing frame of the 150m/min speed of a motor vehicle to singe to weaving face fabric tow sides, the flame temperature while singing is 1250-1300 ℃, and the progression of singing is 6 grades;
Weaving face fabric is dipped in to amylase, and loose formula is pushed on desizing machine, and with the decatize 35-40 minute of 120-125 ℃, destarch rate is 97%;
Weaving face fabric tow sides are carried out to three washings and twice washing, 70 ℃ of washing temperature, washing time 30-35 minute;
With the roller drying of 80 ℃, then use the drum dry of 160 ℃ again;
Dried weaving face fabric is put into pin stenter and carry out tentering, the humidity in stenter is 8%;
Weaving face fabric after tentering is put into preshrinking machine preshrunk;
At 120-125 ℃ of whole boiling hot sizing 20-25 minute.
Advantage of the present invention and beneficial effect are: a kind of finishing technique of weaving face fabric is provided, and it has adopted pure physical finishing technique, without using chemicals, have reduced pollution.
The specific embodiment
Below in conjunction with embodiment, the specific embodiment of the present invention is further described.Following examples are only for technical scheme of the present invention is more clearly described, and can not limit the scope of the invention with this.
The concrete technical scheme of implementing of the present invention is:
Embodiment 1
A finishing technique for weaving face fabric, comprises the steps:
Adopt the gassing frame of the 150m/min speed of a motor vehicle to singe to weaving face fabric tow sides, the flame temperature while singing is 1250 ℃, and the progression of singing is 6 grades;
Weaving face fabric is dipped in to amylase, and loose formula is pushed on desizing machine, and with the decatizes of 120 ℃ 35 minutes, destarch rate was 97%;
Weaving face fabric tow sides are carried out to three washings and twice washing, 70 ℃ of washing temperature, washing time 30 minutes;
With the roller drying of 80 ℃, then use the drum dry of 160 ℃ again;
Dried weaving face fabric is put into pin stenter and carry out tentering, the humidity in stenter is 8%;
Weaving face fabric after tentering is put into preshrinking machine preshrunk;
120 ℃ of whole boiling hot sizings 20 minutes.
Embodiment 2
A finishing technique for weaving face fabric, comprises the steps:
Adopt the gassing frame of the 150m/min speed of a motor vehicle to singe to weaving face fabric tow sides, the flame temperature while singing is 1300 ℃, and the progression of singing is 6 grades;
Weaving face fabric is dipped in to amylase, and loose formula is pushed on desizing machine, and with the decatizes of 125 ℃ 40 minutes, destarch rate was 97%;
Weaving face fabric tow sides are carried out to three washings and twice washing, 70 ℃ of washing temperature, washing time 35 minutes;
With the roller drying of 80 ℃, then use the drum dry of 160 ℃ again;
Dried weaving face fabric is put into pin stenter and carry out tentering, the humidity in stenter is 8%;
Weaving face fabric after tentering is put into preshrinking machine preshrunk;
125 ℃ of whole boiling hot sizings 25 minutes.
Embodiment 3
A finishing technique for weaving face fabric, comprises the steps:
Adopt the gassing frame of the 150m/min speed of a motor vehicle to singe to weaving face fabric tow sides, the flame temperature while singing is 1280 ℃, and the progression of singing is 6 grades;
Weaving face fabric is dipped in to amylase, and loose formula is pushed on desizing machine, and with the decatizes of 124 ℃ 36 minutes, destarch rate was 97%;
Weaving face fabric tow sides are carried out to three washings and twice washing, 70 ℃ of washing temperature, washing time 32 minutes;
With the roller drying of 80 ℃, then use the drum dry of 160 ℃ again;
Dried weaving face fabric is put into pin stenter and carry out tentering, the humidity in stenter is 8%;
Weaving face fabric after tentering is put into preshrinking machine preshrunk;
124 ℃ of whole boiling hot sizings 23 minutes.
The above is only the preferred embodiment of the present invention; it should be pointed out that for those skilled in the art, do not departing under the prerequisite of the technology of the present invention principle; can also make some improvements and modifications, these improvements and modifications also should be considered as protection scope of the present invention.
Claims (1)
1. the finishing technique of weaving face fabric, is characterized in that, comprises the steps:
Adopt the gassing frame of the 150m/min speed of a motor vehicle to singe to weaving face fabric tow sides, the flame temperature while singing is 1250-1300 ℃, and the progression of singing is 6 grades;
Weaving face fabric is dipped in to amylase, and loose formula is pushed on desizing machine, and with the decatize 35-40 minute of 120-125 ℃, destarch rate is 97%;
Weaving face fabric tow sides are carried out to three washings and twice washing, 70 ℃ of washing temperature, washing time 30-35 minute;
With the roller drying of 80 ℃, then use the drum dry of 160 ℃ again;
Dried weaving face fabric is put into pin stenter and carry out tentering, the humidity in stenter is 8%;
Weaving face fabric after tentering is put into preshrinking machine preshrunk;
At 120-125 ℃ of whole boiling hot sizing 20-25 minute.