CN103480941A - 低压铜导线焊接工艺 - Google Patents

低压铜导线焊接工艺 Download PDF

Info

Publication number
CN103480941A
CN103480941A CN201310402310.1A CN201310402310A CN103480941A CN 103480941 A CN103480941 A CN 103480941A CN 201310402310 A CN201310402310 A CN 201310402310A CN 103480941 A CN103480941 A CN 103480941A
Authority
CN
China
Prior art keywords
welding
copper
copper foil
copper bar
welding gun
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201310402310.1A
Other languages
English (en)
Inventor
周伟
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
HEFEI XINWEI ELECTRIC POWER EQUIPMENT CO Ltd
Original Assignee
HEFEI XINWEI ELECTRIC POWER EQUIPMENT CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by HEFEI XINWEI ELECTRIC POWER EQUIPMENT CO Ltd filed Critical HEFEI XINWEI ELECTRIC POWER EQUIPMENT CO Ltd
Priority to CN201310402310.1A priority Critical patent/CN103480941A/zh
Publication of CN103480941A publication Critical patent/CN103480941A/zh
Pending legal-status Critical Current

Abstract

本发明涉及低压铜导线焊接工艺,包括铜排的预处理、焊枪处理、焊接和修整四个步骤,通过对铜箔与铜排的预处理、焊枪处理、焊接,以及修整四个步骤中,及时修整这一步骤,是为了防止在焊接过程中,出现危害操作人员人身安全的隐患发生,提高安全系数,且本发明,焊接质量得到明显提高。

Description

低压铜导线焊接工艺
技术领域
本发明涉及变压器领域,尤其涉及电压等级在20kV及以下的干式变压器铜箔焊接的低压铜导线焊接工艺。
背景技术
变压器是利用电磁感应的原理来改变交流电压的装置,主要构件是初级线圈、次级线圈和铁芯(磁芯)。主要功能有:电压变换、电流变换、阻抗变换、隔离、稳压(磁饱和变压器)等。按用途可以分为:配电变压器、电力变压器、全密封变压器、组合式变压器、干式变压器、油浸式变压器、单相变压器、电炉变压器、整流变压器等。
现有技术中,变压器内部的低压铜导线一般是采用人工焊接,但是,现有的技术,在焊接过程中,焊接质量差,在后期使用时,会出现很多严重的问题,且焊接时安全系数低,容易产生人身安全隐患。
发明内容
有鉴于此,有必要提供一种防止人身安全隐患,且提高焊接质量的低压铜导线焊接工艺。
本发明是这样实现的,低压铜导线焊接工艺,主要包括以下步骤:
步骤一:铜箔与铜排的预处理;
将铜箔与铜排用砂纸砂平,再用夹力钳把铜箔与铜排夹紧,使用小锤敲平铜箔,使铜箔与铜排紧贴,并且使铜排宽出铜箔3~5mm;
步骤二:焊枪处理;
从右向左移动焊接夹具的操作杆,将焊接夹具移到适当位置,然后将铜排与铜箔固定在焊接铜口下, 调节焊枪的位置,使焊枪上的焊针与铜箔的夹角呈60°~80°;
步骤三:焊接;
按下焊接起弧按钮,调节电流,当出现熔融状态时,再慢慢旋转行走电机按钮,边增大电流边调整行走电机速度,直到铜箔与铜排行走处于稳定状态为止,焊接结束时,按下灭弧按钮,抬起焊枪,按下行电机反向行走按钮,使焊枪后移;
步骤四:修整;
使用锉刀锉平焊边,或者砂轮磨平焊边,使焊接的焊缝平整光滑,无尖角毛刺。
进一步地,在所述步骤二中,焊枪上的焊针与铜箔的夹角呈75°。
进一步地,在所述步骤四中,焊接时,焊针每焊接一次,都使用锉刀或者砂轮修整一下,提高焊接质量。
本发明提供的低压铜导线焊接工艺的优点在于:通过对铜箔与铜排的预处理、焊枪处理、焊接,以及修整四个步骤,由于及时修整,防止在焊接过程中,出现危害操作人员人身安全的隐患发生,提高安全系数,且本发明,焊接质量得到明显提高。
具体实施方式
为了使本发明的目的、技术方案及优点更加清楚明白,以下结合实施例,对本发明进行进一步详细说明。应当理解,此处所描述的具体实施例仅仅用以解释本发明,并不用于限定本发明。
所述低压铜导线焊接工艺,主要包括以下步骤:
步骤一:铜箔与铜排的预处理;
将铜箔与铜排用砂纸砂平,再用夹力钳把铜箔与铜排夹紧,使用小锤敲平铜箔,使铜箔与铜排紧贴,并且使铜排宽出铜箔3~5mm,确保铜箔整体能置于铜排排面上。
步骤二:焊枪处理;
从右向左移动焊接夹具的操作杆,将焊接夹具移到适当位置,然后将铜排与铜箔固定在焊接铜口下, 调节焊枪的位置,使焊枪上的焊针与铜箔的夹角呈60°~80°,通过实践证明,在夹角为75°时,焊接效果最佳。
步骤三:焊接;
按下焊接起弧按钮,调节电流,当出现熔融状态时,再慢慢旋转行走电机按钮,边增大电流边调整行走电机速度,直到铜箔与铜排行走处于稳定状态为止,焊接结束时,按下灭弧按钮,抬起焊枪,按下行电机反向行走按钮,使焊枪后移。
步骤四:修整;
使用锉刀锉平焊边,或者砂轮磨平焊边,使焊接的焊缝平整光滑,无尖角毛刺,焊接时,焊针每焊接一次,都使用锉刀或者砂轮修整一下,提高焊接质量。
通过对铜箔与铜排的预处理、焊枪处理、焊接,以及修整四个步骤,由于及时修整,防止在焊接过程中,出现危害操作人员人身安全的隐患发生,提高安全系数,且本发明,焊接质量得到明显提高。
以上所述仅为本发明的较佳实施例而已,并不用以限制本发明,凡在本发明的精神和原则之内所作的任何修改、等同替换和改进等,均应包含在本发明的保护范围之内。

Claims (3)

1.低压铜导线焊接工艺,其特征在于,主要包括以下步骤:
步骤一:铜箔与铜排的预处理;
将铜箔与铜排用砂纸砂平,再用夹力钳把铜箔与铜排夹紧,使用小锤敲平铜箔,使铜箔与铜排紧贴,并且使铜排宽出铜箔3~5mm;
步骤二:焊枪处理;
从右向左移动焊接夹具的操作杆,将焊接夹具移到适当位置,然后将铜排与铜箔固定在焊接铜口下, 调节焊枪的位置,使焊枪上的焊针与铜箔的夹角呈60°~80°;
步骤三:焊接;
按下焊接起弧按钮,调节电流,当出现熔融状态时,再慢慢旋转行走电机按钮,边增大电流边调整行走电机速度,直到铜箔与铜排行走处于稳定状态为止,焊接结束时,按下灭弧按钮,抬起焊枪,按下行电机反向行走按钮,使焊枪后移;
步骤四:修整;
使用锉刀锉平焊边,或者砂轮磨平焊边,使焊接的焊缝平整光滑,无尖角毛刺。
2.根据权利要求1所述的低压铜导线焊接工艺,其特征在于,在所述步骤二中,焊枪上的焊针与铜箔的夹角呈75°。
3.根据权利要求1所述的低压铜导线焊接工艺,其特征在于,在所述步骤四中,焊接时,焊针每焊接一次,都使用锉刀或者砂轮修整一下,提高焊接质量。
CN201310402310.1A 2013-09-06 2013-09-06 低压铜导线焊接工艺 Pending CN103480941A (zh)