Prior art keywords
welding
affected zone
crack
heat
gouge
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2013101073306A
Other languages
English (en)
Inventor
房政
施光涛
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
China MCC17 Group Co Ltd
Original Assignee
China MCC17 Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by China MCC17 Group Co Ltd filed Critical China MCC17 Group Co Ltd
Priority to CN2013101073306A priority Critical patent/CN103192223A/zh
Publication of CN103192223A publication Critical patent/CN103192223A/zh
Pending legal-status Critical Current

Links

Images

Landscapes

  • Butt Welding And Welding Of Specific Article (AREA)

Abstract

本发明公开了一种中厚板焊接热影响区裂纹的处理方法,其具体技术方案如下:第一步、对热影响区裂纹超声波探伤,检测出裂纹的深度;第二步、钻止裂孔,焊前热处理;第三步、二次焊接;第四步、后热处理、焊缝检测。本发明中厚板焊接热影响区裂纹处理方法的优点是方法简单,操作方便,质量可靠,缩短工期,降低成本。

Description

一种中厚板焊接热影响区裂纹的处理方法
技术领域
本发明属钢结构焊接方法,尤其是一种炉壳等中厚板焊接热影响区裂纹的处理方法。
背景技术
在钢结构施工过程中,经常遇到不同厚度的中厚板构件的组装焊接,由于母材厚度不同、焊缝间隙不一致、焊工选用的焊接参数不统一,焊缝受热不均匀等原因,导致焊接应力过大而产生裂纹,造成返工,影响了结构安装工期。
发明内容
本发明所要解决的技术问题是提出一种中厚板焊接热影响区裂纹的处理方法,方法简单,操作方便,质量可靠,缩短工期,降低成本。
为实现上述目的,本发明一种中厚板焊接热影响区裂纹的处理方法,其具体技术方案如下:
第一步:对热影响区裂纹超声波探伤,先对母材热影响区裂纹进行超声波探伤,检测出裂纹的深度,对裂纹深度≤10mm,采用打磨的方法去除;对裂纹深度>10mm,采用气刨的方法去除;
第二步:钻止裂孔,焊前热处理;气刨之前用磁力钻在焊缝裂纹起始端各延长50mm处钻Φ16mm的止裂孔,以防止气刨时焊缝受热影响裂纹的延伸。气刨之前要进行焊前热处理,对热影响区裂纹和焊缝进行加热,加热温度约为100-150℃;(建议增加:止裂孔钻在什么位置有讲究,气刨前也需预热)
第三步:二次焊接,焊前先在母材内侧预热,预热到100-150℃后用岩棉板保温,然后再预热母材外侧,焊接时一定要连续焊接,并保证焊接速度均匀,对焊缝深度较深,采取多层多道焊接,焊条焊前必须进行烘干,并放置在保温桶中;
第四步:后热处理、焊缝检测,焊接完毕之后立即进行后热处理,对焊缝进行加热,加热温度为250-350℃,然后用保温棉对焊缝进行保温,使其进行缓慢冷却,焊接24小时后,对返修的焊缝进行超声波探伤,若存在裂纹,返回第一步处理。
 所述的一种中厚板焊接热影响区裂纹的处理方法,在气刨之前用磁力钻在焊缝裂纹起始端各延长50mm处钻Φ16mm的止裂孔,以防止气刨时焊缝受热影响裂纹的延伸。
 本发明中厚板焊接热影响区裂纹处理方法的优点是方法简单,操作方便,质量可靠,缩短工期,降低成本。
附图说明
图1是本发明所提出的一种中厚板焊接热影响区裂纹的处理方法各部件设置主视结构示意图。
图2是本发明所提出的一种中厚板焊接热影响区裂纹的处理方法各部件设置左侧视结构示意图。
图中:1、母材  2、裂纹   3、焊缝  4、岩棉板   5、止裂孔。
具体实施方式
参见附图,一种中厚板焊接热影响区裂纹的处理方法,先对母材(1)热影响区裂纹(2)进行超声波探伤,检测出裂纹(2)的深度;对裂纹(2)深度≤10mm,采用打磨的方法去除;对裂纹(2)深度>10mm,采用气刨的方法去除;气刨之前用磁力钻在焊缝裂纹起始端各延长50mm处钻Φ16mm的止裂孔(5),以防止气刨时焊缝(3)受热影响裂纹的延伸;气刨之前要进行焊前热处理,对热影响区裂纹(2)和焊缝(3)进行加热,加热温度约为100-150℃;气刨时遇裂缝(2)深度过深,采用多次气刨,每次气刨深度为10mm左右,直至将裂纹(2)全部刨掉;焊接时,选择经验丰富且焊接技术较好的焊工进行二次焊接,焊前先在母材(1)内侧预热,预热到100-150℃后用岩棉板(4)保温,然后再预热母材(1)外侧;焊接时一定要连续焊接,并保证焊接速度均匀,对焊缝(2)深度较深,采取多层多道焊接,焊条焊前必须进行烘干,并放置在保温桶中;焊接完毕之后立即进行后热处理,对焊缝(2)进行加热,加热温度为250-350℃,然后用岩棉板(4)对焊缝进行保温,使其进行缓慢冷却;焊接24小时后,对返修的焊缝进行超声波探伤。

Claims (2)

1.一种中厚板焊接热影响区裂纹的处理方法,其特征在于具体技术方案如下:
第一步:对热影响区裂纹超声波探伤,先对母材热影响区裂纹进行超声波探伤,检测出裂纹的深度,对裂纹深度≤10mm,采用打磨的方法去除;对裂纹深度>10mm,采用气刨的方法去除;
第二步:钻止裂孔,焊前热处理;气刨之前用磁力钻在焊缝裂纹起始端各延长50mm处钻Φ16mm的止裂孔,以防止气刨时焊缝受热影响裂纹的延伸,气刨之前要进行焊前热处理,对热影响区裂纹和焊缝进行加热,加热温度约为100-150℃;
第三步:二次焊接,焊前先在母材内侧预热,预热到100-150℃后用岩棉板保温,然后再预热母材外侧,焊接时一定要连续焊接,并保证焊接速度均匀,对焊缝深度较深,采取多层多道焊接,焊条焊前必须进行烘干,并放置在保温桶中;
 第四步:后热处理、焊缝检测,焊接完毕之后立即进行后热处理,对焊缝进行加热,加热温度为250-350℃,然后用保温棉对焊缝进行保温,使其进行缓慢冷却,焊接24小时后,对返修的焊缝进行超声波探伤,若存在裂纹,返回第一步处理。
2.根据权利要求1所述的一种中厚板焊接热影响区裂纹的处理方法,其特征在于在气刨之前用磁力钻在焊缝裂纹起始端各延长50mm处钻Φ16mm的止裂孔。
CN2013101073306A 2013-03-29 2013-03-29 一种中厚板焊接热影响区裂纹的处理方法 Pending CN103192223A (zh)

Priority Applications (1)

Application Number Priority Date Filing Date Title
CN2013101073306A CN103192223A (zh) 2013-03-29 2013-03-29 一种中厚板焊接热影响区裂纹的处理方法

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
CN2013101073306A CN103192223A (zh) 2013-03-29 2013-03-29 一种中厚板焊接热影响区裂纹的处理方法

Publications (1)

Publication Number Publication Date
CN103192223A true CN103192223A (zh) 2013-07-10

Family

ID=48715137

Family Applications (1)

Application Number Title Priority Date Filing Date
CN2013101073306A Pending CN103192223A (zh) 2013-03-29 2013-03-29 一种中厚板焊接热影响区裂纹的处理方法

Country Status (1)

Country Link
CN (1) CN103192223A (zh)

Cited By (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN103894702A (zh) * 2014-04-10 2014-07-02 大唐山东电力检修运营有限公司 一种电机转子腹板裂纹焊接修复方法
CN103962739A (zh) * 2014-04-23 2014-08-06 哈尔滨飞机工业集团有限责任公司 一种灰口铸铁裂纹的焊接方法
CN104977354A (zh) * 2015-06-30 2015-10-14 共享铸钢有限公司 一种铸钢件补焊返修高温检测方法
CN105149727A (zh) * 2015-09-24 2015-12-16 共享铸钢有限公司 一种中碳钢铸件缺陷去除方法
CN105252202A (zh) * 2015-09-24 2016-01-20 共享铸钢有限公司 一种带筋板的法兰盘类铸件裂纹缺陷的补焊返修方法
CN106198723A (zh) * 2016-07-07 2016-12-07 江苏方天电力技术有限公司 一种螺栓加热孔内壁裂纹的检测装置及方法
DE102016222013A1 (de) 2015-11-30 2017-06-01 Ford Global Technologies, Llc Stoßfängereinheit für ein Kraftfahrzeug
CN107584230A (zh) * 2017-12-14 2018-01-16 徐州徐工矿山机械有限公司 一种可防止焊缝裂纹延伸的焊接连接结构
CN109641329A (zh) * 2016-08-31 2019-04-16 卡特彼勒公司 再制造预燃室组件的方法

Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1911583A (zh) * 2006-08-23 2007-02-14 四川东风电机厂有限公司 水轮发电机转子支架裂纹补焊方法
CN101053926A (zh) * 2007-05-31 2007-10-17 四川东风电机厂有限公司 轴流转桨式水轮机转轮叶片裂纹处理方法
CN101514430A (zh) * 2009-04-07 2009-08-26 杭州汽轮铸锻有限公司 铬钼钒钢及铬钼钒钢铸件的修补工艺
JP4441641B1 (ja) * 2008-11-25 2010-03-31 国立大学法人名古屋大学 鋼構造物の疲労き裂補修方法
CN102441760A (zh) * 2011-11-07 2012-05-09 山西鼎荣冷弯型钢有限公司 冷弯轧辊焊接修复方法
CN102744553A (zh) * 2012-07-17 2012-10-24 上海中油天宝巴圣钢管有限公司 一种厚壁埋弧焊管焊缝横向裂纹的返修方法

Patent Citations (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN1911583A (zh) * 2006-08-23 2007-02-14 四川东风电机厂有限公司 水轮发电机转子支架裂纹补焊方法
CN101053926A (zh) * 2007-05-31 2007-10-17 四川东风电机厂有限公司 轴流转桨式水轮机转轮叶片裂纹处理方法
JP4441641B1 (ja) * 2008-11-25 2010-03-31 国立大学法人名古屋大学 鋼構造物の疲労き裂補修方法
CN101514430A (zh) * 2009-04-07 2009-08-26 杭州汽轮铸锻有限公司 铬钼钒钢及铬钼钒钢铸件的修补工艺
CN102441760A (zh) * 2011-11-07 2012-05-09 山西鼎荣冷弯型钢有限公司 冷弯轧辊焊接修复方法
CN102744553A (zh) * 2012-07-17 2012-10-24 上海中油天宝巴圣钢管有限公司 一种厚壁埋弧焊管焊缝横向裂纹的返修方法

Cited By (15)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
CN103894702B (zh) * 2014-04-10 2016-04-06 大唐山东电力检修运营有限公司 一种电机转子腹板裂纹焊接修复方法
CN103894702A (zh) * 2014-04-10 2014-07-02 大唐山东电力检修运营有限公司 一种电机转子腹板裂纹焊接修复方法
CN103962739A (zh) * 2014-04-23 2014-08-06 哈尔滨飞机工业集团有限责任公司 一种灰口铸铁裂纹的焊接方法
CN104977354A (zh) * 2015-06-30 2015-10-14 共享铸钢有限公司 一种铸钢件补焊返修高温检测方法
CN105149727A (zh) * 2015-09-24 2015-12-16 共享铸钢有限公司 一种中碳钢铸件缺陷去除方法
CN105252202A (zh) * 2015-09-24 2016-01-20 共享铸钢有限公司 一种带筋板的法兰盘类铸件裂纹缺陷的补焊返修方法
CN105149727B (zh) * 2015-09-24 2017-11-28 共享铸钢有限公司 一种中碳钢铸件缺陷去除方法
US10150437B2 (en) 2015-11-30 2018-12-11 Ford Global Technologies, Llc Bumper unit for a motor vehicle
DE102016222013A1 (de) 2015-11-30 2017-06-01 Ford Global Technologies, Llc Stoßfängereinheit für ein Kraftfahrzeug
DE102016222013B4 (de) * 2015-11-30 2021-01-14 Ford Global Technologies, Llc Stoßfängereinheit für ein Kraftfahrzeug
CN106198723A (zh) * 2016-07-07 2016-12-07 江苏方天电力技术有限公司 一种螺栓加热孔内壁裂纹的检测装置及方法
CN106198723B (zh) * 2016-07-07 2023-07-28 江苏方天电力技术有限公司 一种螺栓加热孔内壁裂纹的检测装置及方法
CN109641329A (zh) * 2016-08-31 2019-04-16 卡特彼勒公司 再制造预燃室组件的方法
CN109641329B (zh) * 2016-08-31 2021-07-16 卡特彼勒公司 再制造预燃室组件的方法
CN107584230A (zh) * 2017-12-14 2018-01-16 徐州徐工矿山机械有限公司 一种可防止焊缝裂纹延伸的焊接连接结构

Similar Documents

Publication Publication Date Title
CN103192223A (zh) 一种中厚板焊接热影响区裂纹的处理方法
CN109604767B (zh) 用于厚板窄间隙gma机器人的智能焊接控制系统及方法
CN102441760B (zh) 冷弯轧辊焊接修复方法
CN109702427B (zh) 一种罐体原复合层腐蚀部位修复处理方法
CN105499762A (zh) 一种避免p92钢焊缝金属微细裂纹的焊接工艺
CN101376192B (zh) 22SiMn2TiB钢铲斗刃的焊接方法
CN104801921A (zh) 大直径缸体内套不锈钢套的方法
CN101307676B (zh) 一种复新超高强度抗变形、防腐油井管及其工艺
CN105414878A (zh) 一种高耐热合金钢铸件缺陷的返修方法
CN105312742A (zh) 一种焊接工艺
CN105855786A (zh) 超厚壁管道焊接缺陷的修复方法
CN101699021A (zh) 摩擦焊接式方钻杆
CN105234525B (zh) 一种船体结构钢与锻钢立对接焊接方法
CN103452491B (zh) 一种油田用钻油套管的生产工艺
RU2511191C1 (ru) Способ многослойной сварки труб
CN107414405B (zh) 自升式钻井平台的轴承座焊接裂纹的修补工艺
CN103481008B (zh) 一种深孔焊补工艺
CN104801835A (zh) 一种抗冰隔水管接头不清根焊接方法
CN103962739A (zh) 一种灰口铸铁裂纹的焊接方法
CN102294571A (zh) 高温高压钢管的制造方法
CN104139230A (zh) Q345c钢在超低温下焊接的保温系统及其焊接施工方法
CN104526254A (zh) 四辊卷板机机架断裂的焊接修复方法
CN104439767A (zh) 一种防止风口大套与炉壳焊接出现裂纹的焊接方法
CN105195861B (zh) 一种船体结构钢与锻钢仰对接焊接方法
CN212398558U (zh) 一种钻杆管体和钻杆接头的摩擦焊焊接端面结构

Legal Events

Date Code Title Description
C06 Publication
PB01 Publication
C10 Entry into substantive examination
SE01 Entry into force of request for substantive examination
C02 Deemed withdrawal of patent application after publication (patent law 2001)
WD01 Invention patent application deemed withdrawn after publication

Application publication date: 20130710