CN102953279A - Manufacturing method of household textile fabric - Google Patents
Manufacturing method of household textile fabric Download PDFInfo
- Publication number
- CN102953279A CN102953279A CN 201110239478 CN201110239478A CN102953279A CN 102953279 A CN102953279 A CN 102953279A CN 201110239478 CN201110239478 CN 201110239478 CN 201110239478 A CN201110239478 A CN 201110239478A CN 102953279 A CN102953279 A CN 102953279A
- Authority
- CN
- China
- Prior art keywords
- household textile
- textile fabric
- carried out
- resist agent
- household
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
The invention discloses a manufacturing method of a household textile fabric. The method comprises the steps that: (1) a pretreatment is carried out, wherein the household textile fabric is sequentially subjected to pulp removing, refining, mercerizing and bleaching process treatments; (2) printing is carried out, wherein the pretreated household textile fabric is printed according to designed patterns, and the household textile fabric is sequentially subjected to steaming, washing, and bake-drying treatments; (3) waxing is carried out, wherein the printed fabric is uniformly coated by using a reserving agent; (4) broken-line dyeing is carried out, wherein the household textile fabric coated with the reserving agent is subjected to 2 times of broken-line treatments under a temperature of 0-15 DEG C, and conventional dyeing is then carried out; and (5) post-treatment is carried out, wherein the dyed household textile fabric is subjected to a reserving-agent-removing treatment by using 60-90 DEG C hot water, the printed household textile fabric is then subjected to once or twice soap washing under a temperature of 30-50 DEG C and once or twice washing under room temperature; and the dyed household textile fabric is bake-dried, such that the household textile fabric is obtained. The manufacturing method provided by the invention is simple. The prepared household textile fabric has the advantages of good crease resistance, low cost, suitability for market popularization, and the like.
Description
Technical field
The present invention relates to a kind of manufacture method of household textile lining.
Background technology
The method for making more complicated of general household textile lining, it is bad to make the household textile lining wrinkle resistance that comes, and cost is also high, is unfavorable for the popularization in market.
Summary of the invention
The objective of the invention is provides a kind of manufacture method of simple household textile lining in order to overcome above deficiency.
Purpose of the present invention is achieved through the following technical solutions: a kind of manufacture method of household textile lining, it is characterized in that, and may further comprise the steps:
(1) pre-treatment: household textile lining is carried out boil off, refining, mercerising and bleaching process successively process;
(2) stamp: the household textile lining after pre-treatment is pressed the layout stamp; And warp successively
Evaporate, washing and drying and processing;
(3) wax: printing the even resist agent that applies on the fabric of spending; Described resist agent is following matter
The mixing solidfied material of amount percentage prescription: paraffin: plasticizer SS-202=(90-10): (10-90); The technological temperature of described coating resist agent is 60-100 ℃, and the resist agent consumption is 200-400g/ rice weight fabric;
(4) broken line dyeing: the household textile lining that is coated with resist agent is carried out 2 broken lines process under 0-15 ℃, normal dyeing then,
(5) post processing: adopt 60-90 ℃ hot water to remove resist agent to the household textile lining after the dyeing and process, through 1-2 30-50 ℃ soap and the washing of 1-2 room temperature, then dry and get final product again.
The present invention has the following advantages: method for making is simple, and it is good to make the household textile lining wrinkle resistance that comes, and cost is also low, is beneficial to the popularization in market.
The specific embodiment:
In order to deepen the understanding of the present invention, the invention will be further described below in conjunction with embodiment, and this embodiment only is used for explaining the present invention, does not consist of the restriction to protection domain of the present invention.
The present invention shows a kind of manufacture method of household textile lining, it is characterized in that, may further comprise the steps:
(1) pre-treatment: household textile lining is carried out boil off, refining, mercerising and bleaching process successively process;
(2) stamp: the household textile lining after pre-treatment is pressed the layout stamp; And warp successively
Evaporate, washing and drying and processing;
(3) wax: printing the even resist agent that applies on the fabric of spending; Described resist agent is following matter
The mixing solidfied material of amount percentage prescription: paraffin: plasticizer SS-202=(90-10): (10-90); The technological temperature of described coating resist agent is 60-100 ℃, and the resist agent consumption is 200-400g/ rice weight fabric;
(4) broken line dyeing: the household textile lining that is coated with resist agent is carried out 2 broken lines process under 0-15 ℃, normal dyeing then,
(5) post processing: adopt 60-90 ℃ hot water to remove resist agent to the household textile lining after the dyeing and process, through 1-2 30-50 ℃ soap and the washing of 1-2 room temperature, then dry and get final product again.
The present invention has the following advantages: method for making is simple, and it is good to make the household textile lining wrinkle resistance that comes, and cost is also low, is beneficial to the popularization in market.
Claims (1)
1. the manufacture method of a household textile lining is characterized in that, may further comprise the steps:
(1) pre-treatment: household textile lining is carried out boil off, refining, mercerising and bleaching process successively process;
(2) stamp: the household textile lining after pre-treatment is pressed the layout stamp; And warp successively
Evaporate, washing and drying and processing;
(3) wax: printing the even resist agent that applies on the fabric of spending; Described resist agent is the mixing solidfied material of following mass percent prescription: paraffin: plasticizer SS-202=(90-10): (10-90); The technological temperature of described coating resist agent is 60-100 ℃, and the resist agent consumption is 200-400g/ rice weight fabric;
(4) broken line dyeing: the household textile lining that is coated with resist agent is carried out 2 broken lines process under 0-15 ℃, then normal dyeing;
(5) post processing: adopt 60-90 ℃ hot water to remove resist agent to the household textile lining after the dyeing and process, through 1-2 30-50 ℃ soap and the washing of 1-2 room temperature, then dry again.