CN102942872A - Natural environmentally-friendly paint and preparation method thereof - Google Patents

Natural environmentally-friendly paint and preparation method thereof Download PDF

Info

Publication number
CN102942872A
CN102942872A CN 201110234235 CN201110234235A CN102942872A CN 102942872 A CN102942872 A CN 102942872A CN 201110234235 CN201110234235 CN 201110234235 CN 201110234235 A CN201110234235 A CN 201110234235A CN 102942872 A CN102942872 A CN 102942872A
Authority
CN
China
Prior art keywords
natural
weight
parts
oil
paint
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 201110234235
Other languages
Chinese (zh)
Inventor
徐建辉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Individual
Original Assignee
Individual
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Individual filed Critical Individual
Priority to CN 201110234235 priority Critical patent/CN102942872A/en
Publication of CN102942872A publication Critical patent/CN102942872A/en
Pending legal-status Critical Current

Abstract

The invention relates to paint and especially relates to natural environmentally-friendly paint and a preparation method thereof. The natural environmentally-friendly paint is prepared from 8 to 15 parts by weight of cannabis resin, 5 to 15 parts by weight of loquat oil, 5 to 15 parts by weight of turpentine, 10 to 25 parts by weight of Chinese parasol oil, 2 to 10 parts by weight of polysiloxane, 5 to 25 parts by weight of a natural pigment and 2 to 10 parts by weight of natural filling mountain flour. The natural environmentally-friendly paint has the advantages of rich paint film textures, good water resistance, good elasticity, good flexibility, good chemical resistance, good wear resistance, strong adhesion, high hiding rate, large unit coating area, low use cost, good environmental benefits and no pollution.

Description

Natural environmental-protective paint and preparation method thereof
Technical field
The present invention relates to a kind of paint, especially relate to plant paint of a kind of natural environmental-protective and preparation method thereof.
Background technology
When people mentioned this material of paint of coating, the sensation that readily recognizes that was exactly the decorative coating material that is processed into industrial chemicals, and it has pungent peculiar smell, contains the objectionable impurities composition.Since the man invented paint of coating, do not break away from the category of chemical industry on the basis, it the performance decoration functions in, the invasion and attack that also bring objectionable impurities to people.1, benzene compound mainly evaporates from paint, and benzene,toluene,xylene is indispensable solvent in the paint.2, the additive of various paints and thinner.Benzene exists in the organic solvent of various building and ornament materials in a large number, and such as the solvent or diluent that is commonly called as Tianna solution in the finishing, main component all is benzene,toluene,xylene.3, various tackiness agent.Particularly solvent-based adhesive still has certain market at decoration industry, and use therein solvent majority is toluene, wherein contains the benzene more than 30%, but because the reasons such as price, solvability, cementability are also adopted by some enterprises.The sofa that some families buy discharges a large amount of benzene, and major cause is to have used aborning to contain the high tackiness agent of benzene.4, water-proof material.Particularly some add the waterproof paint that solvent or diluent is mixed with former powder, operate detection in rear 15 hours, and Indoor Air Benzene content surpasses 14.7 times of country's permission maximum concentration.5, some coating low-grade and personation also are the major reasons that causes the Indoor Air Benzene content overproof.Which objectionable impurities in paint and the coating has endanger to human body, and 1, Chronic Benzene Poisoning, mainly be that benzene has hormesis to skin, eyes and the upper respiratory tract.2, suck for a long time benzene and can cause aplastic anemia.3, the women is responsive than the male sex to benzene and homologue harm thereof, and toluene, dimethylbenzene also have certain influence to reproductive function.4, benzene can cause the birth defects of fetus.Along with civilization and progress and scientific development, people are making great efforts aspect the exploration research and development non-polluting coatings paint all the time.
Summary of the invention
The present invention proposes for the problems referred to above, and purpose just provides a kind of nontoxic, pollution-free and play that gloss is beautiful, water-fast, anticorrosion, scratch resistant, the natural environmental-protective of antiultraviolet effect paint.
In order to solve the problems of the technologies described above, the present invention is achieved in that
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=8~15:5~15:5~15:10~25:2~10:5~25:2~10.
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=10~14:8~10:8~10:15~20:5~8:10~20:4~6.
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=12:9:9:18:6:15:5.
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=14:8:9:16:7:17:4.
The preparation method of natural environmental-protective paint of the present invention comprises the steps:
Component is poured in the polyreaction pot, adjusted the tung oil acid number, make acid number reach pH=6.7-6.9; Maintain the temperature between 35 ℃-50 ℃, add coloring material for mixing; Component mixture is ground, and then packing is finished product.
The present invention's effect that compared with prior art has the following advantages: Environmental Safety, technological operation is simple, need not dilution, need not bottoming, stir, directly be coated with once infiltrating covering timber to twice, timber can freely be breathed, reduced harmomegathus and the bending of timber, and played that gloss is beautiful, water-fast, anticorrosion, scratch resistant, the antiultraviolet effect.Use this material brushing at metope, furniture surface, when volatilizing in the brushing operation and after the brushing, can not produce any harm to human body.The color material and the thinner that are used for this paint of coating also are to be extracted by natural phant, do not contain volatile harmful gas.This paint of coating not only has stronger sticking power, and free from extraneous odour, can construct under closed environment, can live in after the brushing.Even residual material volatilizees away, also be to come back in the Nature to circulate, can not produce harmful material.
Embodiment
Embodiment 1
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=8:5:6:10:4:5:2.
The preparation method of natural environmental-protective paint of the present invention comprises the steps: component is poured in the polyreaction pot, adjusts the tung oil acid number, makes acid number reach pH=6.7-6.9; Maintain the temperature between 35 ℃-50 ℃, add coloring material for mixing; Component mixture is ground, and then packing is finished product.
Embodiment 2
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=15:15:15:25:10:25:10.The other the same as in Example 1.
Embodiment 3
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=14:10:10:20:8:20:6.The other the same as in Example 1.
Embodiment 4
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=12:8:9:16:6:15:5.The other the same as in Example 1.
Embodiment 5
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=10:8:8:15:5:10:4.The other the same as in Example 1.
Embodiment 6
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=14:8:9:16:7:17:4.The other the same as in Example 1.
Embodiment 7
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=8:6:7:13:3:13:8.The other the same as in Example 1.
Embodiment 8
Natural environmental-protective paint is to count ratio by following raw materials in parts by weight to be prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=13:15:13:22:7:23:9.The other the same as in Example 1.

Claims (5)

1. a natural environmental-protective paint it is characterized in that counting ratio by following raw materials in parts by weight is prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=8~15:5~15:5~15:10~25:2~10:5~25:2~10.
2. natural environmental-protective paint according to claim 1 it is characterized in that counting ratio by following raw materials in parts by weight is prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=10~14:8~10:8~10:15~20:5~8:10~20:4~6.
3. natural environmental-protective paint according to claim 1 it is characterized in that counting ratio by following raw materials in parts by weight is prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=12:9:9:18:6:15:5.
4. natural environmental-protective paint according to claim 1 it is characterized in that counting ratio by following raw materials in parts by weight is prepared from: hashish: loquat oil: rosin: Chinese parasol tree oil: polysiloxane: natural pigment: natural filling out property stone flour=12:9:9:18:6:15:5.
5. make the method for claim 1,2 or 3 natural environmental-protectives paint:
Component is poured in the polyreaction pot, adjusted the tung oil acid number, make acid number reach pH=6.7-6.9; Maintain the temperature between 35 ℃-50 ℃, add coloring material for mixing; Component mixture is ground, and then packing is finished product.
CN 201110234235 2011-08-16 2011-08-16 Natural environmentally-friendly paint and preparation method thereof Pending CN102942872A (en)