CN102911652A - 一种雾化钻井用阳离子聚合物防塌剂 - Google Patents

一种雾化钻井用阳离子聚合物防塌剂 Download PDF

Info

Publication number
CN102911652A
CN102911652A CN2012104249033A CN201210424903A CN102911652A CN 102911652 A CN102911652 A CN 102911652A CN 2012104249033 A CN2012104249033 A CN 2012104249033A CN 201210424903 A CN201210424903 A CN 201210424903A CN 102911652 A CN102911652 A CN 102911652A
Authority
CN
China
Prior art keywords
monomer
drilling well
cationic polymers
sloughing agent
drilling
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2012104249033A
Other languages
English (en)
Other versions
CN102911652B (zh
Inventor
孙举
王中华
苏雪霞
郝纪双
宋亚静
杨海
马文英
刘光成
杨国涛
国安平
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Drilling Engineering Technology Research Institute Of Zhongyuan Petroleum Exploration Bureau Sinopec
China Petroleum and Chemical Corp
Original Assignee
Drilling Engineering Technology Research Institute Of Zhongyuan Petroleum Exploration Bureau Sinopec
China Petroleum and Chemical Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Drilling Engineering Technology Research Institute Of Zhongyuan Petroleum Exploration Bureau Sinopec, China Petroleum and Chemical Corp filed Critical Drilling Engineering Technology Research Institute Of Zhongyuan Petroleum Exploration Bureau Sinopec
Priority to CN201210424903.3A priority Critical patent/CN102911652B/zh
Publication of CN102911652A publication Critical patent/CN102911652A/zh
Application granted granted Critical
Publication of CN102911652B publication Critical patent/CN102911652B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明涉及一种雾化钻井用阳离子聚合物防塌剂,由有机酰胺类单体A、N-取代酰胺类单体B、阳离子单体C按(60~80):(10~20):(10~20)的质量百分比,在引发剂和pH值调节剂的作用下共聚而成。本发明制备工艺简单,操作方便,所得产品0.5%水溶液72h二次页岩回收率大于90%、饱和吸附量大于100.0mg/g,产品具有强抑制、强吸附的能力,作为雾化钻井流体的防塌剂,能够有效抑制泥页岩的水化膨胀,提高雾化钻井井壁稳定性,延长雾化安全作业时间,充分发挥气体钻井技术优势。

Description

一种雾化钻井用阳离子聚合物防塌剂
技术领域:
本发明涉及一种雾化钻井用阳离子聚合物防塌剂,属于高分子材料制备领域,特别是涉及一种雾化钻井用防塌剂。
背景技术:
雾化钻井是在气体钻井钻遇地层水采用的技术手段,能有效解决地层出水后的钻具泥包、卡钻等问题。但是雾化钻井技术存在井壁稳定时间短,安全作业时间仅为3~5d。雾化钻井属于欠平衡钻井,需从化学的角度提高雾化钻井流体的抑制防塌能力,抑制泥页岩的水化膨胀。国内外雾化钻井一般是选用水基钻井液所用的防塌剂。国外空气雾化钻井最初主要借助所加起泡剂自身的水化抑制性或再添加KCl来稳定井壁;80年代以后选用聚合物稳定剂,主要为聚丙烯酰胺、聚阴离子纤维素、聚丙烯酸酯及阳离子聚胺等。国内空气雾化钻井使用的雾化防塌剂种类单一,主要包括KCl、大分子包被剂、含阳离子单体的聚合物防塌剂等。专利CN101747878A介绍了一种雾化泡沫液,防塌剂为抗高温硅氟防塌剂;专利CN101906294A介绍了气体钻井地层出水条件下井壁保护剂,主要为甲基硅醇钾、水解聚丙烯钠盐和硅酸钠的复合物。此类防塌剂须平衡钻井液抑制性与钻井液胶体稳定性之间的矛盾,因而其抑制能力有限。
发明内容:
本发明内容的目的在于解决现有雾化钻井技术中存在的井壁稳定时间短、抑制防塌能力不足的缺陷,提供了一种抑制防塌性能好,制备工艺简单,成本低的雾化钻井用阳离子聚合物防塌剂。
本发明是通过下述技术方案加以实现:
本发明由有机酰胺类单体A、N-取代酰胺类单体B、阳离子单体C按(60~80):(10~20):(10~20)的质量百分比,在引发剂和pH值调节剂的作用下共聚而成。
上述有机酰胺类单体A为丙烯酰胺、甲基丙烯酰胺中的一种或两种。
上述N-取代丙烯酰胺类单体B为N,N-二甲基丙烯酰胺、N-异丙基丙烯酰胺中的一种或两种。
上述阳离子单体C为二甲基二烯丙基氯化铵、烯丙基三甲基氯化铵、甲基丙烯酰氧乙基三甲基氯化铵中的一种或两种。
所述的引发剂是氧化还原引发剂,氧化剂是过硫酸钾或过硫酸铵的一种,还原剂是亚硫酸氢钠。
所述聚合物防塌剂是由以下步骤制备的:将有机酰胺类单体A、N-取代酰胺类单体B、阳离子单体C按照(60~80):(10~20):(10~20)的质量配比溶于适量水中,通过40%的氢氧化钠溶液调节pH值在9.0~11.0,不断搅拌下慢慢加入引发剂,引发温度在20~60℃,反应时间0.5~2h,产物经剪切造粒,于60℃下烘干、粉碎,即得。
本发明的有益效果是制备工艺简单,操作方便,所得产品0.5%水溶液72h二次页岩回收率大于90%、饱和吸附量大于100.0mg/g,产品具有强抑制、强吸附的能力,作为雾化钻井流体的防塌剂,能够有效抑制泥页岩的水化膨胀,提高雾化钻井井壁稳定性,延长雾化安全作业时间,充分发挥气体钻井技术优势。
具体实施方式:
实施例1:150g水中加入70g丙烯酰胺、20g N,N-二甲基丙烯酰胺,10g二烯丙基二甲基氯化铵,充分溶解后用40%的氢氧化钠溶液调节pH值至9,分别加入0.5g过硫酸铵和0.5g亚硫酸氢钠,在30℃下反应时间0.5h,得到凝胶聚合物,经剪切、造粒,于60℃下烘干、粉碎,得雾化钻井用阳离子聚合物防塌剂。
实施例2:100g水中加入60g丙烯酰胺、15g N,N-二甲基丙烯酰胺,5g N异丙基丙烯酰胺,10g二烯丙基二甲基氯化铵,10g甲基丙烯酰氧乙基三甲基氯化铵,充分溶解后用40%的氢氧化钠溶液调节pH值至10,分别加入0.5g过硫酸铵和0.5g亚硫酸氢钠,在20℃下反应时间1h,得到凝胶聚合物,经剪切、造粒,于60℃下烘干、粉碎,得雾化钻井用阳离子聚合物防塌剂。
实施例3:120g水中加入70g丙烯酰胺,15gN-异丙基丙烯酰胺,15g二烯丙基二甲基氯化铵,充分溶解后用40%的氢氧化钠溶液调节pH值至11,分别加入0.5g过硫酸铵和0.5g亚硫酸氢钠,在60℃下反应时间2h,得到凝胶聚合物,经剪切、造粒,于60℃下烘干、粉碎,得雾化钻井用阳离子聚合物防塌剂。
其他具体实施例按照表1给出组分进行配制。
表1具体实施例组分列表(单位:g)
Figure BDA00002333508700021
Figure BDA00002333508700031
表2实施例的性能指标
Figure BDA00002333508700032
由表2可知,本发明0.5%水溶液72h二次页岩回收率大于90%,饱和吸附量高于100mg/g,常温下溶解性好,抑制防塌能力强。

Claims (6)

1.一种雾化钻井用阳离子聚合物防塌剂,其特征是:由有机酰胺类单体A、N-取代酰胺类单体B、阳离子单体C按(60~80):(10~20):(10~20)的质量百分比,在引发剂和pH值调节剂的作用下共聚而成。
2.根据权利要求1所述的一种雾化钻井用阳离子聚合物防塌剂,其特征是:所述有机酰胺类单体A为丙烯酰胺、甲基丙烯酰胺中的一种或两种。
3.根据权利要求1所述的一种雾化钻井用阳离子聚合物防塌剂,其特征是:所述N-取代酰胺类单体B为N,N-二甲基丙烯酰胺、N-异丙基丙烯酰胺中的一种或两种。
4.根据权利要求1所述的一种雾化钻井用阳离子聚合物防塌剂,其特征是:所述阳离子单体C为二甲基二烯丙基氯化铵、烯丙基三甲基氯化铵、甲基丙烯酰氧乙基三甲基氯化铵中的一种或两种。
5.根据权利要求1所述的一种雾化钻井用阳离子聚合物防塌剂,其特征是:所述的引发剂是氧化还原引发剂,氧化剂是过硫酸钾或过硫酸铵的一种,还原剂是亚硫酸氢钠。
6.根据权利要求1所述的一种雾化钻井用阳离子聚合物防塌剂,其特征是:所述聚合物防塌剂是由以下步骤制备的:将有机酰胺类单体A、N-取代酰胺类单体B、阳离子单体C按照(60~80):(10~20):(10~20)的质量配比溶于适量水中,通过40%的氢氧化钠溶液调节pH值在9.0~11.0,不断搅拌下慢慢加入引发剂,引发温度在20~60℃,反应时间0.5~2h,产物经剪切造粒,于60℃下烘干、粉碎,即得。
CN201210424903.3A 2012-10-30 2012-10-30 一种雾化钻井用阳离子聚合物防塌剂 Active CN102911652B (zh)