CN102677537A - Anti-counterfeiting coating with colored concealed variable patterns for paper and method for preparing colored anti-counterfeiting coating - Google Patents

Anti-counterfeiting coating with colored concealed variable patterns for paper and method for preparing colored anti-counterfeiting coating Download PDF

Info

Publication number
CN102677537A
CN102677537A CN2012101153560A CN201210115356A CN102677537A CN 102677537 A CN102677537 A CN 102677537A CN 2012101153560 A CN2012101153560 A CN 2012101153560A CN 201210115356 A CN201210115356 A CN 201210115356A CN 102677537 A CN102677537 A CN 102677537A
Authority
CN
China
Prior art keywords
parts
paper
color
colored
patterns
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2012101153560A
Other languages
Chinese (zh)
Other versions
CN102677537B (en
Inventor
苏承莲
阚付勤
李寿云
高位肖
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangdong Qiaosheng New Material Technology Co ltd
Original Assignee
DONGGUAN QIAOSHENG PAPER CO LTD
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by DONGGUAN QIAOSHENG PAPER CO LTD filed Critical DONGGUAN QIAOSHENG PAPER CO LTD
Priority to CN201210115356.0A priority Critical patent/CN102677537B/en
Publication of CN102677537A publication Critical patent/CN102677537A/en
Application granted granted Critical
Publication of CN102677537B publication Critical patent/CN102677537B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention relates to anti-counterfeiting coating with colored concealed variable patterns for paper and a method for preparing the anti-counterfeiting coating. The anti-counterfeiting coating comprises, by mass, from 2 to 6 parts of light calcium carbonate, from 3.5 to 8.5 parts of activated clay, from 15 to 25 parts of PD (polyether diols) starch adhesive, from 1.7 to 7.5 parts of antifoaming agent, from 7.5 to 12.5 parts of wheat starch, from 2 to 6 parts of resin color-developing agent, from 7.5 to 12.5 parts of styrene butadiene latex, from 2 to 6 parts of microcapsule color former, from 0.02 to 0.06 part of fluorescer, from 4 to 8 parts of thermochromic materials and from 26 to 36 parts of water. The prepared coating is coated on a paper surface so that anti-counterfeiting paper with colored concealed variable patterns is formed, at the moment, the colored concealed variable patterns have the color of the thermochromic materials and are changed to be colorless when the paper is heated to a certain temperature, the original color of the patterns is recovered after the paper is cooled down, and change of the color is obvious and speedy. In addition, if certain pressure is exerted to the colored concealed variable patterns, the concealed color-changing patterns can be displayed, but the color of the patterns at the stressed position is not changed along with temperature, and the original colored patterns are recovered at unstressed positions.

Description

Paper is with coloured latent change pattern anti-fake coating and manufacturing approach thereof
Technical field
The present invention relates to a kind of coating and manufacturing approach thereof, relate in particular to a kind of paper with coloured latent change pattern anti-fake coating and manufacturing approach thereof.
Background technology
False proof bill is mainly accomplished by body paper manufacturing, coating processing, printing three phases.If at above-mentioned three phases anti-counterfeiting technology is arranged all preferably and form composite anti-fake, antifalse effect will be best, because the fake producer will crack the composite anti-fake technology, just must get together many-sided talent simultaneously, grasps multiple technologies, have multiple equipment.So, the action of fraud strengthens, and exposes easily, and the fraud cost rises significantly, even does not have profit and scheme, and then reduces the generation of imitation behavior.
In the prior art, watermark, safety line technology are only arranged in paper-making process, the very high false tickets of fidelity had taken place in, and latter's cost is very high, is difficult to practicality; At printing stage, various smooth alternating temperatures become fluorescent ink can be purchased everywhere, and the printing house much more extremely to make the antiforge effect relatively poor; At present, the anti-counterfeit paint that does not have high technology content temporarily.
Because counterfeit raising with correlation technique; Paper such as bill, marketable securities, certificate certificate, sign sign require also increasingly high with the anti-counterfeiting technology of product; In order to satisfy this requirement, the anti-counterfeit paint that before the printing of paper articles for use, increases a kind of high-tech of coating becomes present problem demanding prompt solution.
Summary of the invention
To above-mentioned shortcoming, the technical issues that need to address of the present invention provide a kind of paper with coloured latent change pattern anti-fake coating and manufacturing approach thereof.
For achieving the above object, the technical scheme that the present invention adopts is: a kind of paper is with coloured latent change pattern anti-fake coating, and its preparation raw material comprises the component of the quality proportioning that is described below: 2~6 parts of precipitated calcium carbonates; 3.5~8.5 parts of atlapulgites; 15~25 parts of PD amylans; 1.7~7.5 parts of antifoaming agents; 7.5~12.5 parts of wheaten starches; 2~6 parts of resin color-developing agents; 7.5~12.5 parts of styrene-butadiene latexes; 2~6 parts of microcapsules colour formers; 0.02~0.06 part of fluorescer; Temperature becomes 4~8 parts of materials; 26~36 parts in water.
First preferred version of the present invention, above-mentioned paper are with coloured latent change pattern anti-fake coating, and its preparation raw material comprises the component of the quality proportioning that is described below: 4 parts of precipitated calcium carbonates; 5.5 parts of atlapulgites; 20 parts of PD amylans; 5.6 parts of antifoaming agents; 10.5 parts of wheaten starches; 4 parts of resin color-developing agents; 10.5 parts of styrene-butadiene latexes; 4 parts of microcapsules colour formers; 0.04 part of fluorescer; Temperature becomes 6 parts of materials; 30 parts in water.
Second preferred version of the present invention, the color change interval that said temperature becomes material is-15~70 ℃.
Further, according to the manufacturing approach of above-mentioned paper, may further comprise the steps with coloured latent change pattern anti-fake coating:
(1) in material-compound tank, adds entry, start to stir, when stirring, add the PD amylan, pass through heat temperature raising to 90~95 ℃ then, kept temperature 30 minutes, be cooled to 50~60 ℃ again;
When (2) material-compound tank in above-mentioned steps (1) stirs successively to wherein adding precipitated calcium carbonate, atlapulgite, antifoaming agent, wheaten starch, resin color-developing agent, butadiene-styrene latex, microcapsules colour former;
(3) add fluorescer, temperature change material in the material-compound tank of continuation in above-mentioned steps (2) successively, stir, can obtain described paper with coloured latent change pattern anti-fake coating.
Advantage of the present invention: the coating that configures is applied on the paper, and forms coloured latent change pattern anti-fake paper, and this moment, coloured latent change pattern was the color that temperature becomes material; Be heated when reaching uniform temperature; Pattern becomes colorless, and recovers original colored pattern after the cooling again, and change color is obvious and rapid; If apply certain pressure at coloured latent change pattern place, this pattern can show the latent pattern that becomes color, but the pattern place here can the variable color with variation of temperature, and original colored pattern is then recovered in the place of not exerting pressure.
The specific embodiment
In order to deepen to understanding of the present invention, will combine embodiment and accompanying drawing that the present invention is made further detailed description below, this embodiment only is used to explain the present invention, does not constitute the qualification to protection domain of the present invention.
Embodiment 1
Paper may further comprise the steps with the manufacturing approach of coloured latent change pattern anti-fake coating:
(1) take by weighing the preparation raw material, and its preparation raw material comprises the component of the quality proportioning that is described below: 2 parts of precipitated calcium carbonates; 3.5 parts of atlapulgites; 15 parts of PD amylans; 1.7 parts of antifoaming agents; 7.5 parts of wheaten starches; 2 parts of resin color-developing agents; 7.5 parts of styrene-butadiene latexes; 2 parts of blue microcapsules colour formers; 0.02 part of fluorescer; Red temperature becomes 4 parts of materials, 40 ℃ of discoloring temperatures; 26 parts in water;
(2) in material-compound tank, add entry, start to stir, when stirring, add the PD amylan, pass through heat temperature raising to 90 ℃ then, kept temperature 30 minutes, be cooled to 50 ℃ again;
When (3) material-compound tank in above-mentioned steps (2) stirs successively to wherein adding precipitated calcium carbonate, atlapulgite, antifoaming agent, wheaten starch, resin color-developing agent, butadiene-styrene latex, blue microcapsules colour former;
(4) add fluorescer, red temperature change material in the material-compound tank of continuation in above-mentioned steps (3) successively, stir, can obtain described paper with coloured latent change pattern anti-fake coating.
The above-mentioned coating that configures is applied on the page, forms one side on the page and have coloured latent change security pattern, this moment, the finished paper pattern was red; When page is heated when reaching 40 ℃, pattern is become colorless by redness, recovers red after the cooling again immediately; Change color is obvious and rapid, but repeated validation; When being placed UV-irradiation, page can present the blue-fluorescence pattern, but also repeated validation; If apply certain pressure at the red pattern place, this pattern can demonstrate the latent blueness that becomes, and this blueness pattern can the variable color with variation of temperature, and the red pattern of not exerting pressure then still can become colorless with variation of temperature.
Embodiment 2
As another embodiment, different with embodiment 1 is, the preparation raw material that takes by weighing is according to the component of the quality proportioning that is described below: 4 parts of precipitated calcium carbonates; 5.5 parts of atlapulgites; 20 parts of PD amylans; 5.6 parts of antifoaming agents; 10.5 parts of wheaten starches; 4 parts of resin color-developing agents; 10.5 parts of styrene-butadiene latexes; 4 parts of black microcapsules colour formers; 0.04 part of fluorescer; Green temperature becomes 6 parts of materials, and discoloring temperature is 50 ℃; 30 parts in water; Above-mentioned raw materials is configured to coating according to the method for embodiment 1, is applied to then on the page, form one side on the page and have coloured latent change security pattern; This moment, the finished paper pattern was green; When page is heated when reaching 40 ℃, pattern is become colorless by green, recovers green after the cooling again immediately; Change color is obvious and rapid, but repeated validation; When being placed UV-irradiation, page can present the black phosphor pattern, but also repeated validation; If apply certain pressure at green pattern place, this pattern can demonstrate the latent black that becomes, and this black pattern can the variable color with variation of temperature, and the green pattern of not exerting pressure then still can become colorless with variation of temperature.

Claims (4)

1. a paper is with coloured latent change pattern anti-fake coating, and its characteristic is being that its preparation raw material comprises the component of the quality proportioning that is described below: 2~6 parts of precipitated calcium carbonates; 3.5~8.5 parts of atlapulgites; 15~25 parts of PD amylans; 1.7~7.5 parts of antifoaming agents; 7.5~12.5 parts of wheaten starches; 2~6 parts of resin color-developing agents; 7.5~12.5 parts of styrene-butadiene latexes; 2~6 parts of microcapsules colour formers; 0.02~0.06 part of fluorescer; Temperature becomes 4~8 parts of materials; 26~36 parts in water.
2. paper according to claim 1 is characterized in that with coloured latent change pattern anti-fake coating its preparation raw material comprises the component of the quality proportioning that is described below: 4 parts of precipitated calcium carbonates; 5.5 parts of atlapulgites; 20 parts of PD amylans; 5.6 parts of antifoaming agents; 10.5 parts of wheaten starches; 4 parts of resin color-developing agents; 10.5 parts of styrene-butadiene latexes; 4 parts of microcapsules colour formers; 0.04 part of fluorescer; Temperature becomes 6 parts of materials; 30 parts in water.
According to claim 1 or the described paper of claim 2 with coloured latent change pattern anti-fake coating, it is characterized in that the color change interval that said temperature becomes material is-15~70 ℃.
According to claim 1 or the described paper of claim 2 with the manufacturing approach of coloured latent change pattern anti-fake coating, it is characterized in that, may further comprise the steps:
(1) in material-compound tank, adds entry, start to stir, when stirring, add the PD amylan, pass through heat temperature raising to 90~95 ℃ then, kept temperature 30 minutes, be cooled to 50~60 ℃ again;
When (2) material-compound tank in above-mentioned steps (1) stirs successively to wherein adding precipitated calcium carbonate, atlapulgite, antifoaming agent, wheaten starch, resin color-developing agent, butadiene-styrene latex, microcapsules colour former;
(3) add fluorescer, temperature change material in the material-compound tank of continuation in above-mentioned steps (2) successively, stir, can obtain described paper with coloured latent change pattern anti-fake coating.
CN201210115356.0A 2012-04-19 2012-04-19 Anti-counterfeiting coating with colored concealed variable patterns for paper and method for preparing colored anti-counterfeiting coating Active CN102677537B (en)