CN102531456A - 免煅烧工业副产石膏干混砂浆激发剂 - Google Patents

免煅烧工业副产石膏干混砂浆激发剂 Download PDF

Info

Publication number
CN102531456A
CN102531456A CN2012100645727A CN201210064572A CN102531456A CN 102531456 A CN102531456 A CN 102531456A CN 2012100645727 A CN2012100645727 A CN 2012100645727A CN 201210064572 A CN201210064572 A CN 201210064572A CN 102531456 A CN102531456 A CN 102531456A
Authority
CN
China
Prior art keywords
parts
mixed mortar
industry
dry
exciting agent
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN2012100645727A
Other languages
English (en)
Other versions
CN102531456B (zh
Inventor
赵同习
张培清
任春燕
王爱民
王庆珍
赵兵
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shandong Chenghua Building Materials Technology Co ltd
Original Assignee
Jinan High-Tech Area Industrial Waste Utilization Research & Development Center
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Jinan High-Tech Area Industrial Waste Utilization Research & Development Center filed Critical Jinan High-Tech Area Industrial Waste Utilization Research & Development Center
Priority to CN 201210064572 priority Critical patent/CN102531456B/zh
Publication of CN102531456A publication Critical patent/CN102531456A/zh
Application granted granted Critical
Publication of CN102531456B publication Critical patent/CN102531456B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种免煅烧工业副产石膏干混砂浆激发剂,属于干混砂浆添加剂领域。该干混砂浆激发剂由以下重量配比的配料混合制成:氯化钙10—25份、亚硝酸钙3—8份、三乙醇胺5—15份、三异丙醇胺5—15份、工业糖渣30—50份、水10—30份及若干份石粉。与现有技术相比,本发明的干混砂浆激发剂具有适用范围广、不返碱、能够提高砂浆各个龄期强度等特点。

Description

免煅烧工业副产石膏干混砂浆激发剂
技术领域
本发明涉及干混砂浆添加剂领域,具体地说是一种免煅烧工业副产石膏干混砂浆激发剂。
背景技术
目前工业副产石膏的主要品种有火电厂产生的脱硫石膏、磷化工厂产生的磷石膏、氟化工厂产生的氟石膏、柠檬化工厂产生的柠檬化工石膏、钛白化工厂产生的钛石膏等等,对这些石膏的利用主要是煅烧以后做石膏制品,这种利用方法一是耗能并产生新的污染,二是煅烧成本过高和质量不过关;近几年陆续开发出了免煅烧利用工业副产石膏生产干混砂浆技术,其主要原理就是利用激发剂激发相关材料的活性,目前比较有效的通用激发剂主要有:明矾、硫酸钠、硫酸铝、硅酸钠等单用或组合。这些都是固体,其最大的缺点是分散不均匀、因不宜快速溶解而不能充分发挥作用、适用范围窄、效果差、表面泛碱等;这些传统激发剂还会降低砂浆的后期强度;且这些传统的含SO3的激发剂还会延缓砂浆的凝结时间。
发明内容
本发明的技术任务是针对上述现有技术的不足,提供一种免煅烧工业副产石膏干混砂浆激发剂。该激发剂中含有大量液体组份,且其固体组份分散均匀,具有适用范围广、不返碱、能够提高砂浆各个龄期强度等特点。
本发明的技术任务是按以下方式实现的:免煅烧工业副产石膏干混砂浆激发剂,由以下重量配比的配料混合制成:
氯化钙           10—25份
亚硝酸钙         3—8份
三乙醇胺         5—15份
三异丙醇胺             5—15份
工业糖渣         30—50份
水                      10—30份
石粉                              若干份;
将氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺及工业糖渣用水溶解得到中间溶液,以1:9的重量比将中间溶液缓缓加入石粉中,边加入边机械搅拌,搅拌均匀既得目标激发剂。
所述氯化钙为无水氯化钙。
所述三乙醇胺为工业级85混胺。
所述工业糖渣为蔗糖糖渣,糖度为48,锤度为70。
所述石粉目数细于200目,可以选用公知的各种石料的粉末,如石制品加工生产过程中产生的石粉;碎石、人工砂加工生产过程中产生的石粉等等。
本发明将对副产石膏砂浆里的水泥、粉煤灰、副产石膏等具有活性的物质有激发作用的氯化钙等激发剂用水溶解混合均匀,然后用极细石粉作载体,将液体激发剂粉体化,使液体激发剂也可以用于干混砂浆。与现有技术相比具有以下突出的有益效果:
(一)各组分充分溶解且分散均匀,易于溶解分散,能更为有效地发挥激发作用,适用范围广;
(二)本发明的激发剂中不含钠、钾离子,避免了砂浆表面的泛碱现象;
(三)使用了大量的工业糖渣做激发剂,不仅实现了资源综合利用,生态环保,由于工业糖渣对砂浆的各个龄期强度都有增强作用,砂浆的各个龄期强度也都有提高;
(四)由于氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺的存在,缩短了砂浆的凝结时间。
具体实施方式
以具体实施例、实验例对本发明的免煅烧工业副产石膏干混砂浆激发剂作以下详细地说明。
实施例一:
配方:
无水氯化钙 15g                亚硝酸钙 5g                  三乙醇胺 15g
三异丙醇胺 5g                  工业糖渣 40g                水 20g
细于200目的石粉 900g
所述三乙醇胺为工业级85混胺;
所述蔗糖糖渣的糖度为48左右,锤度为70左右。
制备方法:
将配方量的无水氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺及蔗糖糖渣用水溶解,得到中间溶液,以1:9的重量比将中间溶液缓缓加入石粉中,边加入边机械搅拌,搅拌均匀既得目标激发剂。
实施例二:
配方:
无水氯化钙 20g                亚硝酸钙 4g                  三乙醇胺 10g
三异丙醇胺 10g                工业糖渣30g            水 26g
细于200目的石粉 900g
所述三乙醇胺为工业级85混胺;
所述蔗糖糖渣的糖度为48,锤度为70。
制备方法:
将配方量的无水氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺及蔗糖糖渣用水溶解,得到中间溶液,以1:9的重量比将中间溶液缓缓加入石粉中,边加入边机械搅拌,搅拌均匀既得目标激发剂。
实施例三:
配方:
无水氯化钙 15g                亚硝酸钙 7g                  三乙醇胺 5g
三异丙醇胺5g                    工业糖渣 45g                 水 23g
细于200目的石粉 900g
所述三乙醇胺为工业级85混胺;
所述蔗糖糖渣的糖度为48,锤度为70。
制备方法:
将配方量的无水氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺及蔗糖糖渣用水溶解,得到中间溶液,以1:9的重量比将中间溶液缓缓加入石粉中,边加入边机械搅拌,搅拌均匀既得目标激发剂。
对比实验例一:
以下列配方的免煅烧脱硫石膏砂浆为基础配方,将实施例一所得激发剂0.5Kg(除去石粉,有效含量为0.05Kg)与传统激发剂明矾0.05Kg作比较。
配方:
普硅水泥425#:10Kg                             脱硫石膏:20 Kg
机制砂:65Kg                             保水剂(羟丙基甲基纤维素):0.07Kg 
粉煤灰:5Kg                    激发剂:0.5 Kg
实验结果如表1所示。
表1:
Figure 656345DEST_PATH_IMAGE001
对比实验例二:
以下列配方的免煅烧磷石膏砂浆为基础配方,将实施例二所得激发剂0.5Kg(除去石粉,有效含量为0.05Kg)与传统明矾、硫酸铝复合激发剂0.05Kg(复合比例为1:1)作比较。
配方:
普硅水泥425#:10Kg                      磷石膏:20 Kg
机制砂:65 Kg                   保水剂(羟丙基甲基纤维素):0.07Kg   
粉煤灰:5Kg                  激发剂:0.5Kg
实验结果如表2所示。
表2:
Figure 331040DEST_PATH_IMAGE002
对比实验例三:
以下列配方的免煅烧钛石膏砂浆为基础配方,将实施例三所得激发剂0.5Kg(除去石粉,有效含量为0.05Kg)与传统明矾、硫酸铝、硅酸钠复合激发剂0.05Kg(比例为1:1:3)作比较。
配方:
普硅水泥425#:10Kg                                                  钛石膏:20 Kg
机制砂:65 Kg                               激发剂:0.5Kg
保水剂(羟丙基甲基纤维素):0.07Kg               粉煤灰:5Kg
实验结果如表3所示。
表3:
Figure 2012100645727100002DEST_PATH_IMAGE004A

Claims (3)

1.免煅烧工业副产石膏干混砂浆激发剂,其特征在于:由以下重量配比的配料混合制成:
氯化钙            10—25份
亚硝酸钙          3—8份
三乙醇胺          5—15份
三异丙醇胺        5—15份
工业糖渣          30—50份
水                   10—30份
石粉                     若干份;
将氯化钙、亚硝酸钙、三乙醇胺、三异丙醇胺及工业糖渣用水溶解得到中间溶液,以1:9的重量比将中间溶液缓缓加入石粉中,边加入边机械搅拌,搅拌均匀既得目标激发剂。
2.根据权利要求1所述的免煅烧工业副产石膏干混砂浆激发剂,其特征在于:所述工业糖渣为蔗糖糖渣,糖度为48,锤度70。
3.根据权利要求1所述的免煅烧工业副产石膏干混砂浆激发剂,其特征在于:所述石粉目数细于200目。
CN 201210064572 2012-03-13 2012-03-13 免煅烧工业副产石膏干混砂浆激发剂 Active CN102531456B (zh)