CN102430890B - 一种航空发动机外涵道观察窗螺纹脱扣的修复方法 - Google Patents

一种航空发动机外涵道观察窗螺纹脱扣的修复方法 Download PDF

Info

Publication number
CN102430890B
CN102430890B CN 201110278256 CN201110278256A CN102430890B CN 102430890 B CN102430890 B CN 102430890B CN 201110278256 CN201110278256 CN 201110278256 CN 201110278256 A CN201110278256 A CN 201110278256A CN 102430890 B CN102430890 B CN 102430890B
Authority
CN
China
Prior art keywords
observation window
outer duct
welding
thread
thread trip
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 201110278256
Other languages
English (en)
Other versions
CN102430890A (zh
Inventor
任武
王福德
陈继清
李旭照
齐歆霞
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Shenyang Liming Aero Engine Group Co Ltd
Original Assignee
Shenyang Liming Aero Engine Group Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Shenyang Liming Aero Engine Group Co Ltd filed Critical Shenyang Liming Aero Engine Group Co Ltd
Priority to CN 201110278256 priority Critical patent/CN102430890B/zh
Publication of CN102430890A publication Critical patent/CN102430890A/zh
Application granted granted Critical
Publication of CN102430890B publication Critical patent/CN102430890B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种航空发动机外涵道观察窗螺纹脱扣的修复方法,属于发动机修理技术领域。本发明可避免造成浪费和制约生产。本发明包括如下步骤:步骤一:用砂轮打磨掉或用车床车掉外涵道观察窗的螺纹脱扣部位,打磨过程中要保证打磨面或车削面与基体的垂直度和平面度;步骤二:按照步骤一中打磨掉或车掉的外涵道观察窗的螺纹脱扣部位加工一个镶套,用于代替原螺纹脱扣部位;步骤三:用氩弧焊将镶套与观察窗切除后的剩余部位采用对接焊的方法进行焊接;步骤四:用着色对焊缝进行检查,不允许有裂纹,并用原台观察窗的堵盖检查能否顺利安装;步骤五:对外涵道进行工厂试车验证,验证后对焊缝着色检查,着色检查合格,允许装机使用。

Description

一种航空发动机外涵道观察窗螺纹脱扣的修复方法
技术领域
本发明属于发动机修理技术领域,特别是涉及一种航空发动机外涵道观察窗螺纹脱扣的修复方法。
背景技术
航空发动机外涵道是发动机外部的主要承力部件,承担着发动机轴向传力,负荷较大。在发动机大修过程中,发现外涵道观察窗螺纹由于长期使用或安装堵盖时乱扣造成螺纹脱扣,导致整个外涵道不能使用。
目前,当外涵道观察窗螺纹脱扣时,由于没有修复方法而使整台外涵道报废。这就需要整台外涵道更换新品或串件,严重制约生产,并且每台外涵道价值9.8万美元,造成很大的浪费。
发明内容
针对现有技术存在的问题,本发明提供一种可避免造成浪费和制约生产的航空发动机外涵道观察窗螺纹脱扣的修复方法。
为了实现上述目的,本发明采用如下技术方案,一种航空发动机外涵道观察窗螺纹脱扣的修复方法,包括如下步骤:
步骤一:用砂轮打磨掉或用车床车掉外涵道观察窗的螺纹脱扣部位,打磨过程中要保证打磨面或车削面与基体的垂直度和平面度;
步骤二:按照步骤一中打磨掉或车掉的外涵道观察窗的螺纹脱扣部位加工一个镶套,用于代替原螺纹脱扣部位;
步骤三:用氩弧焊将镶套与观察窗切除后的剩余部位采用对接焊的方法进行焊接;
步骤四:用着色对焊缝进行检查,不允许有裂纹,并用原台观察窗的堵盖检查能否顺利安装;
步骤五:对外涵道观察窗进行工厂试车验证,验证后对焊缝再次着色检查,着色检查合格,允许装机使用。
步骤三中所述的对接焊的焊接过程中,选取原台观察窗的堵盖用于镶套与观察窗切除后的剩余部位的定位。
步骤三中所述的氩弧焊的焊接参数如下:
电流种类:直流、正极性,
电流:60A~90A,
焊枪的氩气流量:14L/min~16L/min,
背面吹氩气:8L/min~10L/min,
电极:镧族元素钨Ф2.0mm,
焊丝:TA1Ф1.2mm~1.6mm。
本发明的有益效果:
本发明通过对观察窗的螺纹脱扣部位切除后,然后车加工一个镶套代替原螺纹部位,再用氩弧焊将镶套与观察窗切除后的剩余部位采用对接焊的方法进行焊接;经试验证明:修复后的外涵道观察窗能够装机使用,能够满足发动机修理的技术要求。
本发明创造的经济价值:每台外涵道9.8万美元。
附图说明
图1是修复前具有螺纹脱扣的外涵道观察窗的结构示意图;
图2是本发明的镶套的结构示意图;
图3是打磨或车后外涵道观察窗剩余部位的结构示意图;
图4是采用本发明的修复方法修复后的外涵道观察窗的结构示意图;
图中,1—螺纹脱扣部位,2—外涵道观察窗,3—镶套,4—打磨或车后外涵道观察窗。
具体实施方式
一种航空发动机外涵道观察窗螺纹脱扣的修复方法,包括如下步骤:
步骤一:按设计图尺寸用砂轮打磨掉或用车床车掉外涵道观察窗的螺纹脱扣部位,打磨过程中要保证打磨面或车削面与基体的垂直度和平面度;
步骤二:按照步骤一中打磨掉或车掉的外涵道观察窗的螺纹脱扣部位(如图1所示)加工一个镶套,所述镶套结构如图2所示,用于代替原螺纹脱扣部位;
步骤三:用氩弧焊将镶套与观察窗切除后的剩余部位(如图3所示)采用对接焊的方法进行焊接(如图4所示),对接焊的焊接过程中,选取原台观察窗的堵盖用于镶套与观察窗切除后的剩余部位的定位;
氩弧焊的焊接参数如下:
电流种类:直流、正极性,
电流:60A~90A,
焊枪的氩气流量:14L/min~16L/min,
背面吹氩气:8L/min~10L/min,
电极:镧族元素钨Ф2.0mm;
焊丝:TA1Ф1.2mm~1.6mm;
步骤四:用着色对焊缝进行检查,不允许有裂纹,并用原台观察窗的堵盖检查能否顺利安装;
步骤五:对外涵道观察窗进行工厂试车验证,验证后对焊缝再次着色检查,着色检查合格,允许装机使用。

Claims (3)

1.一种航空发动机外涵道观察窗螺纹脱扣的修复方法,其特征在于,包括如下步骤:
步骤一:用砂轮打磨掉或用车床车掉外涵道观察窗的螺纹脱扣部位,打磨过程中要保证打磨面或车削面与基体的垂直度和平面度;
步骤二:按照步骤一中打磨掉或车掉的外涵道观察窗的螺纹脱扣部位加工一个镶套,用于代替原螺纹脱扣部位;
步骤三:用氩弧焊将镶套与观察窗切除后的剩余部位采用对接焊的方法进行焊接;
步骤四:用着色对焊缝进行检查,不允许有裂纹,并用原台观察窗的堵盖检查能否顺利安装;
步骤五:对外涵道观察窗进行工厂试车验证,验证后对焊缝再次着色检查,着色检查合格,允许装机使用。
2.根据权利要求1所述的一种航空发动机外涵道观察窗螺纹脱扣的修复方法,其特征在于步骤三中所述的对接焊的焊接过程中,选取原台观察窗的堵盖用于镶套与观察窗切除后的剩余部位的定位。
3.根据权利要求1所述的一种航空发动机外涵道观察窗螺纹脱扣的修复方法,其特征在于步骤三中所述的氩弧焊的焊接参数如下:
电流种类:直流、正极性,
电流:60A~90A,
焊枪的氩气流量:14L/min~16L/min,
背面吹氩气:8L/min~10L/min,
电极:镧族元素钨Ф2.0mm,
焊丝:TA1 Ф1.2mm~Ф1.6mm。
CN 201110278256 2011-09-19 2011-09-19 一种航空发动机外涵道观察窗螺纹脱扣的修复方法 Expired - Fee Related CN102430890B (zh)