CN102010736A - 一种替代肥煤的配煤方法 - Google Patents

一种替代肥煤的配煤方法 Download PDF

Info

Publication number
CN102010736A
CN102010736A CN201010583605XA CN201010583605A CN102010736A CN 102010736 A CN102010736 A CN 102010736A CN 201010583605X A CN201010583605X A CN 201010583605XA CN 201010583605 A CN201010583605 A CN 201010583605A CN 102010736 A CN102010736 A CN 102010736A
Authority
CN
China
Prior art keywords
coal
alternative
coking
substitution
substituting
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
CN201010583605XA
Other languages
English (en)
Other versions
CN102010736B (zh
Inventor
薛改凤
付连春
魏松波
项茹
鲍俊芳
陈鹏
常红兵
宋子逵
张前香
张雪红
刘尚超
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Wuhan Iron and Steel Co Ltd
Original Assignee
Wuhan Iron and Steel Group Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Wuhan Iron and Steel Group Corp filed Critical Wuhan Iron and Steel Group Corp
Priority to CN 201010583605 priority Critical patent/CN102010736B/zh
Publication of CN102010736A publication Critical patent/CN102010736A/zh
Application granted granted Critical
Publication of CN102010736B publication Critical patent/CN102010736B/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种替代肥煤的配煤方法,包括如下步骤:获取所用肥煤的粘结指数、膨胀度、最大基氏流动度、挥发份和成焦显微结构组成;确定一种中低变质程度的、粘结指数与所用肥煤的粘结指数相近的、膨胀度和最大基氏流动度及挥发份均大于所用肥煤的一号替代煤种;计算一号替代煤种的替代比例;确定一种成焦显微结构组成与所用肥煤的成焦显微结构组成相近的二号替代煤种;计算二号替代煤种的替代比例;根据一号替代煤种及其替代比例、以及二号替代煤种及其替代比例组合替代所用肥煤。本方法可解决肥煤在炼焦配煤中的可替代问题能节约优质炼焦煤资源,促进焦化行业的可持续发展。

Description

一种替代肥煤的配煤方法
技术领域
本发明涉及炼焦配煤技术领域,具体涉及一种替代肥煤的配煤方法。
背景技术
我国煤资源丰富,但强粘结性的优质炼焦煤资源紧缺。强粘结性的肥煤仅占炼焦煤总量的10%左右,而气煤和1/3焦煤约占炼焦煤总量的46%以上、焦煤占炼焦煤总量的17.57%,瘦煤约占炼焦煤总量的16%。
我国多数焦化企业在配煤炼焦中,肥煤配比一般在20%以上,与占炼焦煤总量的10%左右的肥煤资源量相矛盾,不利于焦化行业的可持续发展。
因此,有必要提供一种在炼焦配煤中肥煤的替代方法来解决肥煤资源量与配煤炼焦中肥煤配比之间的矛盾。
发明内容
本发明的目的是提供一种替代肥煤的配煤方法,解决肥煤资源量与配煤炼焦中肥煤配比之间的矛盾。
为了实现上述目的,本发明提供了一种替代肥煤的配煤方法包括如下步骤:
获取所用肥煤的粘结指数、膨胀度、最大基氏流动度、挥发份和成焦显微结构组成;
确定一种中低变质程度的、粘结指数与所用肥煤的粘结指数相近的、膨胀度和最大基氏流动度及挥发份均大于所用肥煤的一号替代煤种;
计算一号替代煤种的替代比例,计算公式为:X1=Fi(1-|b1-bf|/b1(1-|L1-Lf|/L1)(1-|V1-Vf|/V1),其中,X1为一号替代煤种的替代比例(%),Fi为所用肥煤的配比(%),bf、Lf、Vf分别为所用肥煤的膨胀度、最大基氏流动度、挥发份(%),b1、L1、V1分别为替代煤种1#的膨胀度、最大基氏流动度/挥发份(%);
确定一种成焦显微结构组成与所用肥煤的成焦显微结构组成相近的二号替代煤种;
计算二号替代煤种的替代比例,计算公式为:X2=Fi-X1,其中,X2为二号替代煤种的替代比例(%);
根据一号替代煤种及其替代比例、以及二号替代煤种及其替代比例进行配煤,以替代所用肥煤。
在本发明的一个实施例中,所述一号替代煤种为气肥煤,二号替代煤种为成焦显微结构与所用肥煤相近的1/3焦煤。
经实验,本方法得到的两种煤组合起来能替代肥煤在配煤中的作用,因此本方法可解决肥煤在炼焦配煤中的可替代问题,能节约优质炼焦煤资源,促进焦化行业的可持续发展。
通过以下的描述并结合附图,本发明将变得更加清晰,这些附图用于解释本发明的实施例。
附图说明
图1为本发明替代肥煤的配煤方法的流程图。
具体实施方式
现在参考附图描述本发明的实施例,附图中类似的元件标号代表类似的元件。
如图1,本发明替代肥煤的配煤方法包括如下步骤:
步骤S1,获取所用肥煤的粘结指数、膨胀度、最大基氏流动度、挥发份和成焦显微结构组成;
步骤S2,确定一种中低变质程度的、粘结指数与所用肥煤的粘结指数相近的、膨胀度和最大基氏流动度及挥发份均大于所用肥煤的一号替代煤种;
步骤S3,计算一号替代煤种的替代比例,计算公式为:
X1=Fi(1-|b1-bf|/b1)(1-|L1-Lf|/L1)(1-|V1-Vf|/V1)(1),
其中,X1为一号替代煤种的替代比例(%),
Fi为所用肥煤的配比(%),
bf、Lf、Vf分别为所用肥煤的膨胀度、最大基氏流动度、挥发份(%),
b1、L1、V1分别为替代煤种1#的膨胀度、最大基氏流动度/挥发份(%),
步骤S4,确定一种成焦显微结构组成与所用肥煤的成焦显微结构组成相近的二号替代煤种;
步骤S5,计算二号替代煤种的替代比例,计算公式为:
X2=Fi-X1(2),
其中,X2为二号替代煤种的替代比例(%);
步骤S6,根据一号替代煤种及其替代比例、以及二号替代煤种及其替代比例进行配煤,以替代所用肥煤。
经实验,本发明替代肥煤的方法得到的两种煤组合起来具有较好的流变性、膨胀性,成焦后焦炭显微结构组成中有一定比例的粗粒镶嵌,能替代肥煤在配煤中的作用,因此本方法可解决肥煤在炼焦配煤中的可替代问题,能节约优质炼焦煤资源,促进焦化行业的可持续发展。
需要说明的是,本发明替代肥煤的配煤方法适用于无型煤、无调湿和捣固炼焦的工艺条件。
另外,所述一号煤种可以为气肥煤,所述二号替代煤种可以为成焦显微结构组成与所用肥煤相近的1/3焦煤。
下面以一个具体实例说明本方法组合替代肥煤的原理。
原始配煤方案:
气煤:5%,肥煤20%,1/3焦煤20%,焦煤45%,瘦煤10%。
按此方案配煤在6m焦炉得到的焦炭质量为:抗碎强度(M40):82%,耐磨强度(M10):6.8%,热反应后强度(CSR):64.5%。
上述配煤方案中肥煤用量为20%,本发明方法可以用8%的气肥煤和12%的成焦显微结构与所用肥煤相近的1/3焦煤替代,得到新的配煤方案:
气煤:5%,气肥煤8%,1/3焦煤32%,焦煤45%,瘦煤10%
依此方案配煤在6m焦炉得到的焦炭质量为:抗碎强度(M40):81.5%,耐磨强度(M10):6.3%,热反应后强度(CSR):65.4%。
以上结合最佳实施例对本发明进行了描述,但本发明并不局限于以上揭示的实施例,而应当涵盖各种根据本发明的本质进行的修改、等效组合。

Claims (2)

1.一种替代肥煤的配煤方法,包括如下步骤:
获取所用肥煤的粘结指数、膨胀度、最大基氏流动度、挥发份和成焦显微结构组成;
确定一种中低变质程度的、粘结指数与所用肥煤的粘结指数相近的、膨胀度和最大基氏流动度及挥发份均大于所用肥煤的一号替代煤种;
计算一号替代煤种的替代比例,计算公式为:X1=Fi(1-|b1-bf|b1)(1-|L1-Lf|/L1)(1-|V1-Vf|V1),其中,X1为一号替代煤种的替代比例(%),Fi为所用肥煤的配比(%),bf、Lf、Vf分别为所用肥煤的膨胀度、最大基氏流动度、挥发份(%),b1、L1、V1分别为替代煤种1#的膨胀度、最大基氏流动度/挥发份(%);
确定一种成焦显微结构组成与所用肥煤的成焦显微结构组成相近的二号替代煤种;
计算二号替代煤种的替代比例,计算公式为:X2=Fi-X1,其中,X2为二号替代煤种的替代比例(%);
根据一号替代煤种及其替代比例、以及二号替代煤种及其替代比例组合替代所用肥煤。
2.如权利要求1所述的替代肥煤的配煤方法,其特征在于,所述一号替代煤种为气肥煤,所述二号替代煤种为成焦显微结构组成与肥煤相近的1/3焦煤。
CN 201010583605 2010-12-10 2010-12-10 一种替代肥煤的配煤方法 Active CN102010736B (zh)