CN101537388B - 一种铋钼铜硫混合精矿的分离方法 - Google Patents

一种铋钼铜硫混合精矿的分离方法 Download PDF

Info

Publication number
CN101537388B
CN101537388B CN 200910038844 CN200910038844A CN101537388B CN 101537388 B CN101537388 B CN 101537388B CN 200910038844 CN200910038844 CN 200910038844 CN 200910038844 A CN200910038844 A CN 200910038844A CN 101537388 B CN101537388 B CN 101537388B
Authority
CN
China
Prior art keywords
gram
tons
molybdenum
bismuth
copper
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CN 200910038844
Other languages
English (en)
Other versions
CN101537388A (zh
Inventor
胡真
许志安
陈志强
李汉文
姚建伟
蒋荫林
刘进
张慧
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Guangdong Institute of Resources Comprehensive Utilization
Original Assignee
Guangzhou Research Institute of Non Ferrous Metals
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Guangzhou Research Institute of Non Ferrous Metals filed Critical Guangzhou Research Institute of Non Ferrous Metals
Priority to CN 200910038844 priority Critical patent/CN101537388B/zh
Publication of CN101537388A publication Critical patent/CN101537388A/zh
Application granted granted Critical
Publication of CN101537388B publication Critical patent/CN101537388B/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种铋钼铜硫混合精矿的分离方法。其特征是将铋钼铜硫混合精矿加入活性炭磨矿,调浆,加入矿浆调整剂、抑制剂、捕收剂和起泡剂做钼铜浮选,获得钼铜混合精矿和铋硫混合精矿;钼铜混合精矿加入抑制剂和起泡剂做钼铜分离,获得钼精矿和铜精矿;铋硫混合精矿加入矿浆调整剂、抑制剂、捕收剂和起泡剂做铋硫分离,获得铋精矿和硫精矿。本发明的选矿方法获得的钼精矿钼品位大于45%,钼回收率大于70%,铜精矿铜品位大于20%,铜回收率大于85%,铋精矿铋品位大于24%,铋回收率大于60%,硫精矿硫品位大于35%,硫回收率大于48%。本发明的方法是一种分离效果好,选别指标高的从钼铋铜硫混合精矿中分离钼精矿、铋精矿、铜精矿和硫精矿的方法。

Description

一种铋钼铜硫混合精矿的分离方法
技术领域
本发明涉及一种多金属矿物选矿分离方法,特别涉及一种钼铋铜硫混合精矿的分离方法。
背景技术
铋钼铜硫化矿是一种共生关系复杂的矿物,由于嵌布粒度微细,可浮性相近,分选效果差,特别是铋。处理这一类矿石一般先经浮选作业得到铋钼铜硫混合精矿,再从铋钼铜硫混合精矿中分离钼、铋、铜和硫。分离方法主要有两种:一是重-浮法,即先通过重选获得铋精矿,然后浮选分离钼和铜。但该法分离效果不佳,回收率低,精矿质量不高;二是湿法冶金-浮选法,即首先从铋钼铜硫混合精矿中先浸出铋,通过浸出液回收铋,再浮选浸渣,分离钼和铜,但此方法流程复杂,成本高。
发明目的
本发明的目的是克服现有技术的不足提供的一种分离效果好,选别指标高的从钼铋铜硫混合精矿中分离出钼精矿、铋精矿、铜精矿和硫精矿的方法。本发明的分离方法由以下步骤组成:
(1)磨矿:在铋钼铜硫混合精矿中加入活性炭500~1000克/吨,磨矿至-0.043毫米占90%,浓密脱水;
(2)调浆:加水至矿浆浓度为35~40%;
(3)钼铜浮选:加入矿浆调整剂石灰调节矿浆pH值为11~13,依次加入抑制剂500~800克/吨、捕收剂40~60克/吨和起泡剂150~180克/吨做一次粗选;加入捕收剂20~40克/吨和起泡剂60~80克/吨做一次扫选;加入捕收剂15~25克/吨和起泡剂20~40克/吨做二次扫选;加入抑制剂100~300克/吨和起泡剂10~20克/吨进行一次精选;加入抑制剂50~150克/吨和起泡剂5~10克/吨进行二次精选;再做一次空白精选;获得钼铜混合精矿和铋硫混合精矿;
(4)钼铜分离:加入抑制剂2000~4000克/吨和起泡剂60~80克/吨做一次粗选;加入抑制剂1000~2000克/吨和起泡剂30~40克/吨做一次扫选;加入抑制剂500~1000克/吨和起泡剂30~40克/吨做二次扫选;加入抑制剂1000~2000克/吨做一次精选;加入抑制剂500~1000克/吨做二次精选;获得钼精矿和铜精矿;
(5)铋硫分离:用矿浆调整剂调节矿浆pH值为9~10,加入抑制剂1000~1500克/吨、捕收剂60~80克/吨和起泡剂20克/吨做一次粗选;加入捕收剂30~40克/吨,起泡剂10克/吨做一次扫选;加入捕收剂10~20克/吨和起泡剂5克/吨做二次扫选;加入抑制剂300~500克/吨进行一次精选;再做一次空白精选;获得铋精矿和硫精矿。
所述抑制剂为水玻璃、硫化钠、硫氢化钠或硫酸锌。
所述捕收剂为丁铵黑药、乙硫氮或丁基黄药。
所述起泡剂为煤油、柴油或2号油。
本发明是根据铋钼铜硫化矿在不同pH介质中的可浮性特征,在高碱度的石灰介质中铋受到抑制,而钼和铜仍具有良好的可浮性,使铋与钼和铜分离,在铋浮选前添加硫酸锌和亚硫酸钠抑制黄铁矿,采用硫酸活化受抑制的铋,实现铋和硫的分离。本发明的选矿方法获得的钼精矿钼品位大于45%,钼回收率大于70%,铜精矿铜品位大于20%,铜回收率大于85%,铋精矿铋品位大于24%,铋回收率大于60%,硫精矿硫品位大于35%,硫回收率大于48%。
附图说明
图1为本发明的铋钼铜硫混合精矿分离方法的流程图。
具体实施方式
本发明以某矿山的自然铋钼铜硫化矿为例,原矿含钼0.079%、铜0.28%、铋0.076%,硫2.23%,铋钼铜硫混合精矿含钼0.76%、铜4.28%、铋0.92%,硫16.18%。按常规浮选方法得到铋钼铜硫混合精矿,按照实施例的步骤和表1所列出的药剂用量进行分离。
表1实施例1~3药剂用量(克/吨,铋钼铜硫混合精矿)
Figure G2009100388444D00031
实施例1
(1)磨矿:在钼铋铜硫混合精矿中加入活性炭500克/吨磨至-0.043mm占90%,脱药,浓密脱水;(2)调浆:加水调节矿浆浓度为35%;用石灰调节矿浆pH值为11;(3)钼铜浮选和(4)钼铜分离按表1所列药剂用量操作,得到钼精矿和铜精矿;(5)铋硫分离:用硫酸调节矿浆pH值为9,按表1所列药剂用量操作,得到铋精矿和硫精矿。
得到的钼精矿钼品位为46.87%,钼回收率达到81.56%,含铜0.20%,含铋0.19%,元素化学分析结果列于表2。铜精矿铜品位为21.28%,铜回收率达到93.56%,含钼0.43%,含铋0.46%,元素化学分析结果见表3。得到的铋精矿铋品位为26.96%,铋回收率达到69.09%,含钼0.38%,含铜0.40%,元素化学分析结果见表4。得到的硫精矿硫品位为36.15%,硫回收率达到50.24%,含铜0.06%,含铋0.21%,含钼0.085%,元素化学分析结果见表5。
表2钼精矿元素化学分析结果
Figure G2009100388444D00041
表3铜精矿元素化学分析结果
Figure G2009100388444D00042
表4铋精矿元素化学分析结果
Figure G2009100388444D00043
表5硫精矿元素化学分析结果
实施例2
(1)磨矿:在钼铋铜硫混合精矿中加入活性炭800克/吨磨至-0.043mm占90%,脱药,浓密脱水;(2)调浆:加水调节矿浆浓度为37%;用石灰调节矿浆pH值为12;(3)钼铜浮选和(4)钼铜分离按表1所列药剂用量操作,得到钼精矿和铜精矿;(5)铋硫分离:用硫酸调节矿浆pH值为9,按表1所列药剂用量操作,得到铋精矿和硫精矿。
得到的钼精矿钼品位为45.92%,钼回收率达到79.48%,含铜0.18%,含铋0.21%。铜精矿铜品位为20.43%,铜回收率达到89.68%,含钼0.47%,含铋0.51%。得到的铋精矿铋品位为24.85%,铋回收率达到63.24%,含钼0.47%,含铜0.36%。得到的硫精矿硫品位为35.73%,硫回收率达到49.64%,含铜0.07%,含铋0.22%,含钼0.076%。
实施例3
(1)磨矿:在钼铋铜硫混合精矿中加入活性炭1000克/吨磨至-0.043mm占90%,脱药,浓密脱水;(2)调浆:加水调节矿浆浓度为40%;用石灰调节矿浆pH值13;(3)钼铜浮选和(4)钼铜分离按表1所列药剂用量操作,得到钼精矿和铜精矿;(5)铋硫分离:用硫酸调节矿浆pH值为10,按表1所列药剂用量操作,得到铋精矿和硫精矿。
得到的钼精矿钼品位为46.38%,钼回收率达到73.28%,含铜0.24%,含铋0.18%。铜精矿铜品位为20.67%,铜回收率达到87.95%,含钼0.36%,含铋0.48%。得到的铋精矿铋品位为25.76%,铋回收率达到65.29%,含钼0.41%,含铜0.39%。得到的硫精矿硫品位为37.46%,硫回收率达到48.73%,含铜0.06%,含铋0.19%,含钼0.082%。

Claims (4)

1.一种铋钼铜硫混合精矿的分离方法,其特征是由以下步骤组成:
(1)磨矿:在铋钼铜硫混合精矿中加入活性炭500~1000克/吨,磨矿至-0.043毫米占90%,浓密脱水;
(2)调浆:加水至矿浆浓度为35~40%;
(3)钼铜浮选:加入矿浆调整剂石灰调节矿浆pH值为11~13,依次加入抑制剂500~800克/吨、捕收剂40~60克/吨和起泡剂150~180克/吨做一次粗选;加入捕收剂20~40克/吨和起泡剂60~80克/吨做一次扫选;加入捕收剂15~25克/吨和起泡剂20~40克/吨做二次扫选;加入抑制剂100~300克/吨和起泡剂10~20克/吨进行一次精选;加入抑制剂50~150克/吨和起泡剂5~10克/吨进行二次精选;获得钼铜混合精矿和铋硫混合精矿;
(4)钼铜分离:加入抑制剂2000~4000克/吨和起泡剂60~80克/吨做一次粗选;加入抑制剂1000~2000克/吨和起泡剂30~40克/吨做一次扫选;加入抑制剂500~1000克/吨和起泡剂30~40克/吨做二次扫选;加入抑制剂1000~2000克/吨做一次精选;加入抑制剂500~1000克/吨做二次精选;获得钼精矿和铜精矿;
(5)铋硫分离:用硫酸调节矿浆pH值为9~10,加入抑制剂1000~1500克/吨、捕收剂60~80克/吨和起泡剂20克/吨做一次粗选;加入捕收剂30~40克/吨,起泡剂10克/吨做一次扫选;加入捕收剂10~20克/吨和起泡剂5克/吨做二次扫选;加入抑制剂300~500克/吨进行一次精选;获得铋精矿和硫精矿。
2.根据权利要求1所述的铋钼铜硫混合精矿的分离方法,其特征是所述抑制剂为水玻璃、硫化钠、硫氢化钠或硫酸锌。
3.根据权利要求1所述的铋钼铜硫混合精矿的分离方法,其特征是所 述捕收剂为丁铵黑药、乙硫氮或丁基黄药。
4.根据权利要求1所述的铋钼铜硫混合精矿的分离方法,其特征是所述起泡剂为煤油、柴油或2号油。 
CN 200910038844 2009-04-21 2009-04-21 一种铋钼铜硫混合精矿的分离方法 Expired - Fee Related CN101537388B (zh)