CN101294088A - 一种炼焦煤细分配煤方法 - Google Patents
一种炼焦煤细分配煤方法 Download PDFInfo
- Publication number
- CN101294088A CN101294088A CNA2008100481063A CN200810048106A CN101294088A CN 101294088 A CN101294088 A CN 101294088A CN A2008100481063 A CNA2008100481063 A CN A2008100481063A CN 200810048106 A CN200810048106 A CN 200810048106A CN 101294088 A CN101294088 A CN 101294088A
- Authority
- CN
- China
- Prior art keywords
- coal
- coking
- coking coal
- lean
- blending
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Granted
Abstract
本发明涉及一种炼焦煤细分配煤方法,它包括将参与配煤的炼焦煤混配的步骤,参与配煤的炼焦煤至少包括:焦煤、1/3焦煤、瘦煤;焦煤包括焦煤1#或/和焦煤2#;1/3焦煤包括1/3焦煤1#;瘦煤包括瘦煤1#或/和瘦煤2#;上述炼焦煤占配煤总重量的百分比为:焦煤1#25-50%;焦煤2# 8-25%;1/3焦煤1# 25-45%;瘦煤1# 8-20%;瘦煤2# 5-14%。本发明方法能科学合理的对炼焦煤的煤质进行细分和使用,正确指导配煤炼焦,对炼焦煤做到合理使用,精细配煤。
Description
技术领域
本发明涉及炼焦配煤技术领域,特别是炼焦配煤方法。
背景技术
炼焦煤由于成煤过程和成煤植物不同造成了种类的多样性和基本性质的复杂性。中国地域辽阔,煤源分布广,煤质差异大。相同分类的煤,随地区的不同煤质发生变化;同一地区不同矿点的煤质也不尽相同,同一矿点而不同煤层的煤质量也会发生差异。这种差异在目前炼焦煤国标分类中可能为同一种煤,但会引起焦炭质量的较大波动。
目前,炼焦配煤方法主要是按国标分类的大类煤种——气煤、气肥煤、肥煤、1/3焦煤、焦煤和瘦煤的调整配煤的比例,还不能做到配煤的准确和合理,因为在炼焦配煤中有一些煤种并不能够起到相应煤种的作用,特别是配比较高的焦煤、1/3焦煤和瘦煤,虽然按国家标准都被化为焦煤或1/3焦煤,但在配煤炼焦中,有的能起到相应煤种的作用,有的起到的作用比相应煤种要好,而有的煤根本起不到相应煤种的作用。
为了做到配煤的准确合理,国内许多焦化企业开始对所用的炼焦煤在国标的基础上进行进一步细分亚类,如把焦煤分成焦煤1类、焦煤2类等等,但这类分类方法的科学性和适用性较差。一般采用:1、按煤出产地区细分,但由于同一地区的煤质差异很大,就是同一矿点不同煤层的煤质差异也很大,对于采取配煤办法供煤的矿的煤质质量波动更大;2、用反射率分布图的叠合性进行细分,这种方法适用性较差,在实际工作中很难找到反射率分布图能较好叠合的煤来。
发明内容
本发明所要解决的技术问题是:提供一种炼焦煤细分配煤方法,该方法能科学合理的对炼焦煤的煤质进行细分和使用,正确指导配煤炼焦,对炼焦煤做到合理使用,精细配煤。
本发明解决上述技术问题所采用的技术方案是:
一种炼焦煤细分配煤方法,它包括将参与配煤的炼焦煤混配的步骤,参与配煤的炼焦煤至少包括:焦煤、1/3焦煤、瘦煤;
焦煤包括焦煤1#或/和焦煤2#;其中:焦煤1#为粗粒镶嵌指数≥50%的焦煤,焦煤2#为粗粒镶嵌指数为30-50%的焦煤;
1/3焦煤包括1/3焦煤1#;其中:1/3焦煤1#为镶嵌指数≥70%的1/3焦煤;所述镶嵌指数=粗粒镶嵌指数+细粒镶嵌指数;
瘦煤包括瘦煤1#或/和瘦煤2#;其中:瘦煤1#为粘接指数G值≥40的瘦煤,瘦煤2#为粘接指数G值在20-40的瘦煤;
上述炼焦煤占配煤总重量的百分比为:
焦煤1#25-50%;焦煤2#8-25%;1/3焦煤1#25-45%;
瘦煤1#8-20%;瘦煤2#5-14%。
上述方案中,焦煤还包括焦煤3#;其中:焦煤3#为粗粒镶嵌指数<30%的焦煤;焦煤3#占配煤总重量的百分比为:3-8%。
上述方案中,1/3焦煤还包括1/3焦煤2#或/和1/3焦煤3#;其中:1/3焦煤2#为镶嵌指数在50-70%的1/3焦煤,1/3焦煤3#为镶嵌指数<50%的1/3焦煤;1/3焦煤2#、1/3焦煤3#占配煤总重量的百分比为:
1/3焦煤2#8-20%;1/3焦煤3#3-10%。
上述方案中,焦煤的总重量≤配煤总重量的50%。
上述方案中,1/3焦煤的总重量≤配煤总重量的45%。
上述方案中,瘦煤的总重量≤配煤总重量的20%。
焦炭质量在炼焦工艺一定的情况下,取决于配合煤的结焦性和成焦显微结构组成。本发明方法根据上述原理,克服了现有配煤方法的缺陷,能科学合理的对炼焦煤的煤质进行细分和使用,正确指导配煤炼焦,对炼焦煤做到合理使用,精细配煤,对特定焦炭热性能实现定量配煤。
具体实施方式
本发明炼焦煤细分配煤方法实施例,参与配煤方法的炼焦煤至少包括:焦煤、1/3焦煤、瘦煤;方法包括:
第一步、细分焦煤、1/3焦煤、瘦煤的步骤;该步骤具体包括:
1、对焦煤成焦显微结构进行检测,并按粗粒镶嵌指数细分为:焦煤1#为粗粒镶嵌指数≥50%的焦煤,焦煤2#为粗粒镶嵌指数为30-50%的焦煤,焦煤3#为粗粒镶嵌指数<30%的焦煤。
2、对1/3焦煤成焦显微结构进行检测,并按镶嵌指数细分为:1/3焦煤1#为镶嵌指数≥70%的1/3焦煤,1/3焦煤2#为镶嵌指数在50-70%的1/3焦煤,1/3焦煤3#为镶嵌指数<50%的1/3焦煤;所述镶嵌指数=粗粒镶嵌指数+细粒镶嵌指数;
3、对瘦煤进行检测,并按粘接指数G值细分为:瘦煤1#为粘接指数G值≥40的瘦煤,瘦煤2#为粘接指数G值在20-40的瘦煤。
第二步、将参与配煤的炼焦煤混配的步骤,其中,各炼焦煤占配煤总重量的百分比为:
焦煤1#25-50%;焦煤2#8-25%;焦煤3#3-8%;焦煤的总重量一般不超过配煤总重量的50%,即:焦煤的总重量≤配煤总重量的50%。
1/3焦煤1#25-45%;1/3焦煤2#8-20%;1/3焦煤3#3-10%;1/3焦煤的总重量一般不超过配煤总重量的45%,即:1/3焦煤的总重量≤配煤总重量的45%。
瘦煤1#8-20%;瘦煤2#5-14%。瘦煤的总重量一般不超过配煤总重量的20%,即:瘦煤的总重量≤配煤总重量的20%。
本发明炼焦煤细分配煤方法实施例1-7,参与配煤的炼焦煤原料性质分析如下:
单种煤样 灰分% 挥发分% G Y Rmax 粗粒镶嵌指数 镶嵌指数
气肥煤 8.26 40.84 98 28 0.68
肥煤 9.82 33.26 94 26 0.95
焦煤1# 10.18 23.78 87 18 1.24 65
焦煤2# 10.23 24.24 84 18 1.45 45
焦煤3# 10.32 25.62 76 16 1.21 18.5
1/3焦煤1# 9.36 31.58 89 17 0.90 74
1/3焦煤2# 9.27 36.82 80 15 0.84 60.5
1/3焦煤3# 9.48 35.64 75 14 0.72 44.5
瘦煤1# 9.89 16.78 48 6 1.4 5
瘦煤2# 10.12 15.24 24 3 1.8 6
本发明炼焦煤细分配煤方法实施例1-7,各炼焦煤占配煤总重量的百分比见表1:
表1:
单种煤样 | 实施例1 | 实施例2 | 实施例3 | 实施例4 | 实施例5 | 实施例6 | 实施例7 |
气肥煤 | 4 | 6 | 6 | 0 | 5 | 0 | 9 |
肥煤 | 4 | 5 | 5 | 0 | 3 | 10 | 0 |
焦煤1# | 25 | 45 | 28 | 50 | 25 | 30 | 28 |
焦煤2# | 8 | 0 | 0 | 0 | 10 | 10 | 8 |
焦煤3# | 0 | 0 | 8 | 0 | 0 | 0 | 4 |
1/3焦煤1# | 25 | 25 | 25 | 30 | 44 | 25 | 25 |
1/3焦煤2# | 20 | 0 | 8 | 0 | 0 | 11 | 8 |
1/3焦煤3# | 0 | 7 | 0 | 8 | 0 | 0 | 3 |
瘦煤1# | 0 | 0 | 20 | 0 | 8 | 9 | 8 |
瘦煤2# | 14 | 12 | 0 | 12 | 5 | 5 | 7 |
本发明炼焦煤细分配煤方法实施例1-7得到的配煤,在6米焦炉所得焦炭质量:抗碎强度M40>82%;耐磨强度M10<7.2%;反应性(CRI)<30%,反应后强度(CSR)>62%。
本发明炼焦煤细分配煤方法实施例8,其参与配煤的炼焦煤原料性质分析如下:
单种煤样 灰分% 挥发分% G Y Rmax 粗粒镶嵌指数 镶嵌指数
气肥煤 8.34 43.56 97 27 0.68
1/3焦煤1# 10.2 30.46 86 19 0.94 76
1/3焦煤2# 9.27 34.82 77 15 0.84 58
焦煤1# 10.18 23.78 86 18 1.24 55
瘦煤1# 9.89 16.48 48 6 1.42
各炼焦煤占配煤总重量的百分比:气肥煤7%;1/3焦煤1#30%;1/3焦煤2#8%;焦煤1#38%;瘦煤1#17%。
本发明炼焦煤细分配煤方法实施例8得到的配煤,在6米焦炉所得焦炭质量:抗碎强度M40:82.4%;耐磨强度M10:7.1%;反应性(CRI):28.9%,反应后强度(CSR):64.5%。
本发明炼焦煤细分配煤方法实施例9,其参与配煤的炼焦煤均为国产煤,炼焦煤原料性质分析如下:
单种煤样 灰分% 挥发分% G Y Rmax 粗粒镶嵌指数 镶嵌指数
气肥煤 8.34 43.56 97 27 0.65
肥煤 9.23 32.56 94 26 1.05
1/3焦煤1# 9.36 31.22 89 16 0.78 74
1/3焦煤2# 9.27 34.82 77 15 0.84 58
1/3焦煤3# 9.36 31.22 89 16 0.78 42
焦煤2# 10.23 24.78 80 18 1.18 42
瘦煤2# 10.12 15.24 32 3 1.86
各炼焦煤占配煤总重量的百分比:气肥煤9%;肥煤7%;1/3焦煤1#34%;1/3焦煤2#8%;1/3焦煤3#3%;焦煤2#25%;瘦煤2#14%。
本发明炼焦煤细分配煤方法实施例9得到的配煤,在4.63米焦炉所得焦炭质量:抗碎强度M40:80.18%,耐磨强度M10:7.4%,反应性(CRI):29.8%,反应后强度(CSR):62.5%。
本发明炼焦煤细分配煤方法实施例10,其参与配煤的炼焦煤原料性质分析如下:
单种煤样 灰分% 挥发分% G Y Rmax 粗粒镶嵌指数 镶嵌指数
气肥煤 8.34 43.56 97 27 0.65
肥煤 9.23 32.56 94 26 1.05
1/3焦煤1# 10.2 30.46 86 19 0.94 76
1/3焦煤3# 9.48 35.82 75 14 0.72 44
焦煤1# 10.18 23.78 86 18 1.24 55
焦煤3# 10.32 24.62 72 14 1.14 18
瘦煤1# 10.13 16.18 43 6 1.56
各炼焦煤占配煤总重量的百分比:气肥煤5%;1/3焦煤1#30%;1/3焦煤3#8%;肥煤5%;焦煤1#32%;焦煤3#5%;瘦煤1#15%。
本发明炼焦煤细分配煤方法实施例10得到的配煤,在4.63米焦炉所得焦炭质量:抗碎强度M40:80.12%,耐磨强度M10:7.38%,反应性(CRI):28.8%,反应后强度(CSR):63.1%。
以上分析数据均按照煤分析的国家标准进行分析。
Claims (6)
1、一种炼焦煤细分配煤方法,它包括将参与配煤的炼焦煤混配的步骤,参与配煤的炼焦煤至少包括:焦煤、1/3焦煤、瘦煤;其特征在于:
焦煤包括焦煤1#或/和焦煤2#;其中:焦煤1#为粗粒镶嵌指数≥50%的焦煤,焦煤2#为粗粒镶嵌指数为30-50%的焦煤;
1/3焦煤包括1/3焦煤1#;其中:1/3焦煤1#为镶嵌指数≥70%的1/3焦煤;所述镶嵌指数=粗粒镶嵌指数+细粒镶嵌指数;
瘦煤包括瘦煤1#或/和瘦煤2#;其中:瘦煤1#为粘接指数G值≥40的瘦煤,瘦煤2#为粘接指数G值在20-40的瘦煤;
上述炼焦煤占配煤总重量的百分比为:
焦煤1# 25-50%;焦煤2# 8-25%;1/3焦煤1# 25-45%;
瘦煤1# 8-20%;瘦煤2# 5-14%。
2、如权利要求1所述的方法,其特征在于:焦煤还包括焦煤3#;其中:焦煤3#为粗粒镶嵌指数<30%的焦煤;焦煤3#占配煤总重量的百分比为:3-8%。
3、如权利要求1或2所述的方法,其特征在于:1/3焦煤还包括1/3焦煤2#或/和1/3焦煤3#;其中:1/3焦煤2#为镶嵌指数在50-70%的1/3焦煤,1/3焦煤3#为镶嵌指数<50%的1/3焦煤;1/3焦煤2#、1/3焦煤3#占配煤总重量的百分比为:
1/3焦煤2# 8-20%;1/3焦煤3# 3-10%。
4、如权利要求2所述的方法,其特征在于:焦煤的总重量≤配煤总重量的50%。
5、如权利要求3所述的方法,其特征在于:1/3焦煤的总重量≤配煤总重量的45%。
6、如权利要求1所述的方法,其特征在于:瘦煤的总重量≤配煤总重量的20%。