CN101092728A - Low-foam degreasing powder for cleaning surfaces of steel materials and preparation method thereof - Google Patents

Low-foam degreasing powder for cleaning surfaces of steel materials and preparation method thereof Download PDF

Info

Publication number
CN101092728A
CN101092728A CN 200710021429 CN200710021429A CN101092728A CN 101092728 A CN101092728 A CN 101092728A CN 200710021429 CN200710021429 CN 200710021429 CN 200710021429 A CN200710021429 A CN 200710021429A CN 101092728 A CN101092728 A CN 101092728A
Authority
CN
China
Prior art keywords
parts
content
powder
sodium
preparation
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN 200710021429
Other languages
Chinese (zh)
Inventor
瞿德勤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
JIANGYAN DYMATIC CHEMICALS Inc
Original Assignee
JIANGYAN DYMATIC CHEMICALS Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JIANGYAN DYMATIC CHEMICALS Inc filed Critical JIANGYAN DYMATIC CHEMICALS Inc
Priority to CN 200710021429 priority Critical patent/CN101092728A/en
Publication of CN101092728A publication Critical patent/CN101092728A/en
Pending legal-status Critical Current

Abstract

The invention discloses a low-foam degreasing powder for cleaning the surface of a steel material and a preparation method thereof, wherein the degreasing powder comprises the following components in parts by weight: 28-50 parts of sodium carbonate, 10-30 parts of sodium tripolyphosphate, 20200.2-3 parts of polyether, 2.2-5 parts of an organic silicon defoamer, 8-25 parts of sodium metasilicate pentahydrate, 1-4 parts of disodium and 30-60 parts of sodium hydroxide, wherein the above components are uniformly mixed; the degreasing powder is prepared by mixing sodium carbonate and sodium tripolyphosphate, adding polyether 2020 and organic silicon defoamer, stirring, adding sodium metasilicate pentahydrate, disodium and sodium hydroxide, and stirring to obtain the final product. The degreasing powder has the advantages of super-strong permeability, good cleaning effect, 2-3 times improvement of degreasing and cleaning speed, less foam during use, no toxicity and contribution to human health and environmental protection.

Description

Be used for low foaming spent meal in use of steel material surface cleaning and preparation method thereof
Technical field
The present invention relates to a kind of low foaming spent meal in use that is used for the steel material surface cleaning, and relate to the preparation method of this spent meal.
Background technology
In production processes such as electronic connector plating continuously, tin plating of the steel plate, steel plate hot dip process and color steel chromaking, need carry out the surface to workpiece to be plated to wash down, the quality of cleaning directly influences the outward appearance and the use properties of workpiece.The grease-removing agent that uses in industrial pressure wash at present is because its component, proportioning and preparation method's defective exists cleaning speed slow, and foam is many, and the unfavorable problem of degreasing effect directly influences the rustless property of production efficiency and product.
Summary of the invention
The technical problem to be solved in the present invention provides that a kind of cleaning speed is fast, and foam is few, and degreasing effect is good is used for low foaming spent meal in use that steel material surface cleans and preparation method thereof.
The object of the present invention is achieved like this:
The component and the proportioning that are used for the low foaming spent meal in use of steel material surface cleaning are:
28~50 parts in the yellow soda ash of content 98~99.9%
10~30 parts of tripoly phosphate sodium STPPs
2,020 0.2~3 parts of polyethers
2.2~5 parts of silicone antifoam agents
8~25 parts of the metasilicate pentahydrate sodiums of content 27~29%
1~4 part of disodium
30~60 parts in the sodium hydroxide of content 96~99%
Above proportioning is weight part.
The optimum ratio of the described component of above-mentioned spent meal is:
30~36 parts in the yellow soda ash of content 98~99.9%
13~20 parts of tripoly phosphate sodium STPPs
2,020 0.8~1.5 parts of polyethers
2.8~4 parts of silicone antifoam agents
12~18 parts of the metasilicate pentahydrate sodiums of content 27~29%
2~2.5 parts of disodiums
30~40 parts in the sodium hydroxide of content 96~99%
Above proportioning is weight part.
The preparation method of above-mentioned spent meal carries out as follows:
(1) 28~50 parts in the yellow soda ash of content 98~99.9% is mixed for 10~30 parts with tripoly phosphate sodium STPP, stir the A powder;
(2) 2,020 0.2~3 parts of polyethers mixed with 2.2~5 parts of silicone antifoam agents add the A powder, stir the B powder;
(3) will be after 30~60 parts of mixing of sodium hydroxide of 8~25 parts of the inclined to one side silicon Starsos of five water of content 27~29%, 1~4 part of disodium, content 96~99% add the B powder, stir the finished product low foaming spent meal in use, above proportioning is weight part.
Compared with prior art, the present invention has adopted new raw material, proportioning and preparation method, the low foaming spent meal in use that makes has superpower penetrating power, cleaning performance is good, the oil removing cleaning speed improves 2~3 times than like product, foam is few during use, has solved the many difficult problems of foam in the pressure wash process.And this spent meal is nontoxic, does not contain carcinogenss such as nitrite, and is safe in utilization, helps environment protection.
Embodiment
Further specify the present invention below by embodiment.
Component, consumption such as following table among each embodiment:
Embodiment 1 Embodiment 2 Embodiment 3 Embodiment 4 Embodiment 5 Embodiment 6
Yellow soda ash Content % 98 99.9 99.5 98.5 99 99.2
Consumption kg 50 28 30 36 34 32
Tripoly phosphate sodium STPP kg 30 10 13 20 15 18
Polyethers 2020kg 3 0.2 0.8 1.5 1.0 1.2
Silicone antifoam agent kg 5 2.2 2.8 4 3 3.5
Metasilicate pentahydrate sodium Content % 29 28 27.5 29 28 28.5
Consumption kg 8 25 18 12 16 14
Disodium kg 4 1 2 2.5 2.2 2.4
Sodium hydroxide Content % 99 96 97 98 98.5 97.5
Consumption kg 31 60 40 34 30 38
The preparation method of spent meal all carries out as follows among each embodiment:
(1) yellow soda ash is mixed with tripoly phosphate sodium STPP, stir the A powder;
(2) will polyethers 2020, silicone antifoam agent mixes the back and adds the A powder, stir the B powder;
(3) will metasilicate pentahydrate sodium, disodium, sodium hydroxide mix the back and add the B powder, stir the finished product low foaming spent meal in use.

Claims (3)

1, a kind of low foaming spent meal in use that is used for the steel material surface cleaning, its component and proportioning are:
28~50 parts in the yellow soda ash of content 98~99.9%
10~30 parts of tripoly phosphate sodium STPPs
2,020 0.2~3 parts of polyethers
2.2~5 parts of silicone antifoam agents
8~25 parts of the metasilicate pentahydrate sodiums of content 27~29%
1~4 part of disodium
30~60 parts in the sodium hydroxide of content 96~99%
Above proportioning is weight part.
2, by the described low foaming spent meal in use of claim 1, it is characterized in that the optimum ratio of described component is:
30~36 parts in the yellow soda ash of content 98~99.9%
13~20 parts of tripoly phosphate sodium STPPs
2,020 0.8~1.5 parts of polyethers
2.8~4 parts of silicone antifoam agents
12~18 parts of the metasilicate pentahydrate sodiums of content 27~29%
2~2.5 parts of disodiums
30~40 parts in the sodium hydroxide of content 96~99%
Above proportioning is weight part.
3, a kind of preparation method of low foaming spent meal in use according to claim 1, carry out as follows:
(1) 28~50 parts in the yellow soda ash of content 98~99.9% is mixed for 10~30 parts with tripoly phosphate sodium STPP, stir the A powder;
(2) 2,020 0.2~3 parts of polyethers mixed with 2.2~5 parts of silicone antifoam agents add the A powder, stir the B powder;
(3) will add the B powder after 30~60 parts of mixing of sodium hydroxide of 1~4 part of 8~25 parts of metasilicate pentahydrate sodiums, the disodium of content 27~29%, content 96~99%, stir the finished product low foaming spent meal in use, above proportioning is weight part.
CN 200710021429 2007-04-11 2007-04-11 Low-foam degreasing powder for cleaning surfaces of steel materials and preparation method thereof Pending CN101092728A (en)