CN100544858C - 金属液态压铸锻造双控一次成型的方法 - Google Patents

金属液态压铸锻造双控一次成型的方法 Download PDF

Info

Publication number
CN100544858C
CN100544858C CNB200410052493XA CN200410052493A CN100544858C CN 100544858 C CN100544858 C CN 100544858C CN B200410052493X A CNB200410052493X A CN B200410052493XA CN 200410052493 A CN200410052493 A CN 200410052493A CN 100544858 C CN100544858 C CN 100544858C
Authority
CN
China
Prior art keywords
forging
casting
die
liquid
pressure
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CNB200410052493XA
Other languages
English (en)
Other versions
CN1647871A (zh
Inventor
李远发
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Richwood Industrial Science and Technology (Huizhou) Co., Ltd.
Original Assignee
JIARUI INTERNATIONAL CO Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by JIARUI INTERNATIONAL CO Ltd filed Critical JIARUI INTERNATIONAL CO Ltd
Priority to CNB200410052493XA priority Critical patent/CN100544858C/zh
Publication of CN1647871A publication Critical patent/CN1647871A/zh
Application granted granted Critical
Publication of CN100544858C publication Critical patent/CN100544858C/zh
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

本发明公开了一种金属液态压铸锻造双控一次成型的方法,采用液态铸锻双控一次成型铸锻机,其基本原理是在压力铸造机的基础上附加锻造的功能,把熔料温度为500-800℃的液态金属输入模腔,压力为8-40兆帕,填充速度为0.01-10米/秒,加压锻造开始的时间是在熔化的金属液填满整个模具型腔成型后的0.05-2秒,加压锻造模具的温度为200-350℃,锻造压力为6-30兆帕。采用本发明,在同一个生产周期中对液态金属连续进行压力铸造和模锻一次成型,零件的密度比压铸件的缩孔数量减少10%以上,零件的强度度比压铸件提升10%以上,特别适应生产形状复杂、强度要求高的精密机械零件,质量稳定,成品率高。

Description

金属液态压铸锻造双控一次成型的方法
技术领域
本发明涉及金属压铸成型的方法,特别是一种金属液态压铸锻造双控一次成型的方法。
背景技术
传统的压力铸造的方法是液压金属在高压、高速下充填模具腔铸造的,往往型腔中的气体难以排除干净以及紊流导致铸件内部气孔、缩孔和疏松的产生,特别是压铸形状复杂、强度要求高的精密机械零件如汽车配件的成品率较低。
发明内容
本发明的目的是针对上述的缺点,研究出一种金属液态压铸锻造双控一次成型的方法,可以在同一个生产周期中对液态金属连续进行压力铸造和模锻,特别适应制造形状复杂、强度要求高的精密机械零件,质量稳定,成品率高。
本发明的目的是这样实现的:
采用液态铸锻双控一次成型铸锻机,其基本原理是在压力铸造机的基础上附加锻造的功能,其结构是两个大行程油缸完成合模和后模动作;一个小行程大油缸完成液态或半固态模锻;输送坯料油缸:把液态金属输入至填充模腔;侧缸——合模式加压用。
采用加压锻造模具的结构包括与压铸模具类似的上下模、模框、模芯、滑决、流道和顶出机构外,还包括可以锻造的冲头。其中锻压冲头和模具的间隙大小是非常重要的,过小会造成冲头和模具相碰或卡住,过大会造成飞料。金属液态压铸锻造双控一次成型的工艺流程是采用压力把液态金属输模腔,压力锻造、加压锻造双控一次成型,顶出模腔内一次成型零件。
金属液态压铸锻造双控一次成型的工艺参数如下:
1、液态金属输入模腔压力铸造
控制熔料(液态金属)温度为500-800℃,把液态金属输入至充填模腔的压力为8-40兆帕,填充速度为0.01-10米/秒,液态金属压力锻造成型。以上压力铸造工艺参数的控制将直接影响熔化的金属液是否能填满整个模具型腔,以及金属液中气孔的多少。
2、加压锻造
(1)、加压锻造模具的温度:
控制加压锻造模具的温度为200-350℃,模具温度直接影响零件的质量和模具寿命,本模具加热采用热油加热的方式。
(2)、加压锻造开始的时间:
控制加压锻造开始的时间是在熔化的金属液(液态金属)填满整个模具型腔成型后的0.05-2秒,加压锻造开始的时间对加压锻造效果有很大影响。
(3)、加压锻造的压力:
控制锻造压力为6-30兆帕,锻造压力大小对零件的物理机械性能,织结构有直接影响。
3、顶出零件
后开模具,把锻造后的零件顶出模腔。
由于采用本发明,在同一个生产周期中对液态金属连续进行压力铸造和模锻,零件的密度比压铸件的缩孔数量减少10%以上,零件的强度度比压铸件提升10%以上,特别适应生产形状复杂、强度要求高的精密机械零件,质量稳定,成品率高。
实施方案
结合实施例,进一步描述本发明的方法。
实施例:金属液态压铸锻造双控一次成型制造摩托车发动机外壳
采用液态铸锻双控一次成型铸锻机,其基本原理是在压力铸造机的基础上附加锻造的功能,其结构是两个大行程油缸完成合模和后模的动作;一个小行程大油缸完成液态或半固态模锻;输送坯料油缸:把液态金属输入至充填模腔;侧缸——合模式加压用。
采用加压锻造模具的结构包括与压铸模具类似的上下模、模框、模芯、滑决、流道和顶出机构外,还包括可以锻造的冲头。其中锻压冲头和模具的间隙大小是非常重要的,过小会造成冲头和模具相碰或卡住,过大会造成飞料。
金属液态压铸锻造双控一次成型制造摩托车发动机外壳的工艺如下:
1、液态合金输入模腔压力铸造
控制熔料温度为650℃,把液态合金压入摩托车发动机外壳模腔,压力为10兆帕,填充速度为0.08米/秒,液态金属填满整个模具型腔压力铸造成型。
2、加压锻造
(1)、加压锻造模具的温度:
控制加压锻造模具的温度为300℃,本模具加热采用热油加热的方式。
(2)、加压锻造开始的时间:
控制加压锻造开始的时间是在熔化的金属液填满整个模具型腔成型后的0.05秒。
(3)、加压锻造的压力:
控制锻造压力为10兆帕。
3、顶出零件
后开模具,从模腔中顶出摩托车发动机外壳。

Claims (1)

1.金属液态压铸锻造双控一次成型的方法,采用压力把液态金属输入模腔,其特征是:采用压力把液态金属输入模腔内压力铸造和加压锻造双控一次成型,金属液态压铸锻造双控一次成型的工艺:
A、液态金属输入模腔压力铸造
控制液态金属温度为500-800℃,把液态金属输入模腔的压力为8-40兆帕,填充速度为0.01-10米/秒;
B、加压锻造
(1)、加压锻造模具的温度
控制加压锻造模具的温度为200-350℃;
(2)、加压锻造开始的时间
控制加压锻造开始的时间是在液态金属填满整个模具型腔成型后的0.05-2秒;
(3)、加压锻造的压力
控制锻造压力为6-30兆帕。
CNB200410052493XA 2004-12-03 2004-12-03 金属液态压铸锻造双控一次成型的方法 Active CN100544858C (zh)