CN100419091C - 镁棒炉外铁水脱硫方法 - Google Patents

镁棒炉外铁水脱硫方法 Download PDF

Info

Publication number
CN100419091C
CN100419091C CNB2006100395213A CN200610039521A CN100419091C CN 100419091 C CN100419091 C CN 100419091C CN B2006100395213 A CNB2006100395213 A CN B2006100395213A CN 200610039521 A CN200610039521 A CN 200610039521A CN 100419091 C CN100419091 C CN 100419091C
Authority
CN
China
Prior art keywords
desulfurization
magnesium
magnesium rod
magnesium bar
rifle
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CNB2006100395213A
Other languages
English (en)
Other versions
CN1827791A (zh
Inventor
王朝东
黄晶
吴小江
刁岳川
朱琨
石东
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nanjing Iron and Steel United Co Ltd
Original Assignee
Nanjing Iron and Steel United Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nanjing Iron and Steel United Co Ltd filed Critical Nanjing Iron and Steel United Co Ltd
Priority to CNB2006100395213A priority Critical patent/CN100419091C/zh
Publication of CN1827791A publication Critical patent/CN1827791A/zh
Application granted granted Critical
Publication of CN100419091C publication Critical patent/CN100419091C/zh
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

一种炉外铁水脱硫方法,包括以下步骤:将镁棒固定在脱硫枪体上;在冷确系统的冷却(冷却枪体)和惰性气体的保护下,将镁棒插入铁水缸中;一支镁棒用尽时,更换新的镁棒。具体操作是:在脱硫枪体内安装金属镁棒,在液压保护装置中惰性气体的保护下,液压杠杆将脱硫枪体内的镁棒插入铁水罐中,脱硫反应开始;当脱硫枪体内的镁棒少于20~30mm时,更换新的镁棒;以上步骤反复进行到脱硫过程结束。本发明提供的炉外铁水脱硫方法,克服了传统技术镁粉脱硫工艺的缺点;新方法成本低廉、操作简便,镁棒可以快速更换,同时,还可以使脱硫更加完全。

Description

镁棒炉外铁水脱硫方法
技术领域
本发明属于铁水炉外预处理技术领域,脱硫工艺的改进方法,特别是一种利用镁棒的炉外铁水脱硫方法。
背景技术
铁水炉外脱硫是冶金工业生产的常用技术之一,现有的铁水炉外脱硫技术有以下几种:
石灰石脱硫,也称为KR法脱硫;
镁粉加石灰脱硫;
单纯使用镁粉脱硫,是利用惰性气体的保护将钝化镁粒喷吹至铁水罐中,以达到脱硫的目的。但这种方法容易受镁粒质量的影响,脱硫不完全,而且高纯度的镁粉、镁粒的成本较高,使脱硫工艺的阶段成本过高,不利于该技术的推广。
发明内容
发明目的:本发明为克服上述镁粉脱硫工艺的缺点,将提供一种成本低廉、操作简便的的炉外铁水脱硫方法,该方法在降低成本的同时,还可以使脱硫更加完全。
完成上述发明任务的技术方案是,炉外铁水脱硫方法,包括以下步骤:
将镁棒固定在脱硫枪体上;
在冷确系统的冷却(冷却枪体)和惰性气体的保护下,将镁棒插入铁水缸中;
一支镁棒用尽时,更换新的镁棒。
更具体地说,以上方法的步骤可以是:
待脱硫的铁水由铁水罐经火车送至铁水脱硫工位;
在脱硫枪体内安装金属镁棒,并通过快速连接装置与液压缸连接;
升起并旋转脱硫枪至铁水罐上方;
开通液压缸下部的水冷系统;
打开液压保护装置通入惰性气体;
脱硫枪体下降至预定位置;
液压缸开始工作,在惰性气体的保护下,液压杠杆将脱硫枪体内的镁棒插入铁水罐中,脱硫反应开始;
当脱硫枪体内的镁棒少于20~30mm时,枪体上升,快速回到起始位置,液压杠杆推掉残存的镁棒;
脱硫枪旋转至枪体更换位置,打开快速连接装置,更换新的镁棒;
以上步骤反复进行到脱硫过程结束。
本发明提供的炉外铁水脱硫方法,克服了传统技术镁粉脱硫工艺的缺点;新方法成本低廉、操作简便,镁棒可以快速更换,同时,还可以使脱硫更加完全。
具体实施方式
实施例1,炉外铁水脱硫方法,包括以下步骤:
待脱硫的铁水由铁水罐经火车送至脱硫工位;
在脱硫枪体内安装金属镁棒,并通过快速连接装置与液压缸连接;
升起并旋转脱硫枪至铁水罐上方;
开通液压缸下部的水冷系统;
打开脱硫枪体保护装置通入惰性气体;
脱硫枪体下降至预定位置;
液压缸开始工作,在惰性气体的保护下,夜压杠杆将脱硫枪体内的镁棒推入铁水罐中,脱硫反应开始;
当脱硫枪体内的镁棒少于20~30mm时,枪体上升,快速回到起始位置,液压杠杆推掉残存的镁棒;
脱硫枪旋转至枪体更换位置,打开快速连接装置,更换新的镁棒;以上步骤反复进行到脱硫过程结束。
完成上述工作所使用的设备包括:
铁水缸及防溅罩;
脱硫枪,包括液压推杆,快速连接装置,由枪管和保温材料构成的保温枪体;其上安装的镁棒;
升降机构;
旋转机构;
液压站;
水冷系统;
氮气保护系统;
控制系统;
枪体更换装置。

Claims (1)

1. 一种炉外铁水脱硫方法,包括以下步骤:
将镁棒固定在脱硫枪体上;
在冷却系统的冷却和惰性气体的保护下,将镁棒插入铁水罐中;
一支镁棒用尽时,更换新的镁棒;
以上方法的具体工作步骤是:
待脱硫的铁水由铁水罐经火车送至铁水脱硫工位;
在脱硫枪体内安装金属镁棒,并通过快速连接装置与液压缸连接;
升起并旋转脱硫枪至铁水罐上方;
开通液压缸下部的水冷系统;
打开液压保护装置通入氮气;
脱硫枪体下降至预定位置;
液压缸开始工作,在氮气的保护下,液压杠杆将脱硫枪体内的镁棒插入铁水罐中,脱硫反应开始;
当脱硫枪体内的镁棒少于30mm时,枪体上升,快速回到起始位置,液压杠杆推掉残存的镁棒;
脱硫枪旋转至枪体更换位置,打开快速连接装置,更换新的镁棒;
以上步骤反复进行到脱硫过程结束;
完成上述工作所使用的设备包括:
铁水罐及防溅罩;
脱硫枪,包括液压杠杆,快速连接装置,由枪管和保温材料构成的保温枪体,其上安装的镁棒;
升降机构;
旋转机构;
液压站;
水冷系统;
氮气保护系统;
控制系统;
枪体更换装置。
CNB2006100395213A 2006-04-14 2006-04-14 镁棒炉外铁水脱硫方法 Expired - Fee Related CN100419091C (zh)