AT122012B - Process for accelerating the vulcanization of rubbers. - Google Patents

Process for accelerating the vulcanization of rubbers.

Info

Publication number
AT122012B
AT122012B AT122012DA AT122012B AT 122012 B AT122012 B AT 122012B AT 122012D A AT122012D A AT 122012DA AT 122012 B AT122012 B AT 122012B
Authority
AT
Austria
Prior art keywords
sep
vulcanization
accelerating
rubbers
accelerator
Prior art date
Application number
Other languages
German (de)
Original Assignee
Ig Farbenindustrie Ag
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ig Farbenindustrie Ag filed Critical Ig Farbenindustrie Ag
Application granted granted Critical
Publication of AT122012B publication Critical patent/AT122012B/en

Description

  

   <Desc/Clms Page number 1> 
 



  Verfahren zur Beschleunigung der Vulkanisation von   Xalltschukarten.   
 EMI1.1 
 
 EMI1.2 
 
 EMI1.3 
 Beschleuniger darstellen, die auch   bei geringem Schwefelgehalt 20#25% höhere   Zerreissfestigkeiten der Vulkanisate ergeben. Die als neue Vulkanisatoren erkannten Produkte der vorgenannten Klasse zeigen, dass ausserordentlich starke Beschleuniger vorliegen, die vielfach besser sind als z. B. Diarylguanidine. Die bessere Wirksamkeit der Vulkanisationsbeschleuniger gemäss vorliegender Erfindung ergibt sich aus den folgenden Versuchen : 
1. Versuch : 
 EMI1.4 
 
<tb> 
<tb> Die <SEP> Mischung <SEP> besteht <SEP> aus
<tb> 100-0 <SEP> Teilen <SEP> Gummi.
<tb> 



  3-5. <SEP> Schwefel,
<tb> 5#0 <SEP> ,, <SEP> Zinkweiss,
<tb> 1'0,., <SEP> Beschleuniger.
<tb> 



  Beschleuniger <SEP> 25', <SEP> 35', <SEP> 45' <SEP> bei <SEP> 3 <SEP> 1/2 <SEP> Atü.
<tb> Tolylaminoimidazolin <SEP> 204, <SEP> 182, <SEP> 179 <SEP> kg/cm2 <SEP> Festigkeit
<tb> Diphenylguanidin <SEP> 170,180, <SEP> 183 <SEP> ,, <SEP> ,,
<tb> 
 
 EMI1.5 
 2. Versuch : 
 EMI1.6 
 
<tb> 
<tb> Die <SEP> Mischung <SEP> besteht <SEP> aus
<tb> 100-0 <SEP> Teilen <SEP> Gummi.
<tb> 



  25#0 <SEP> ,, <SEP> Gasruss,
<tb> 5#0 <SEP> ,, <SEP> Zinkweiss.
<tb> 



  3-0 <SEP> Schwefel,
<tb> 1'0 <SEP> " <SEP> Beschleuniger.
<tb> 



  Beschleuniger <SEP> 10', <SEP> 301, <SEP> 601, <SEP> 90' <SEP> bei <SEP> 2# <SEP> Atü.
<tb> Tolylaminoimidazolin <SEP> 108, <SEP> 187, <SEP> 225, <SEP> 204kg/cm3 <SEP> Festigkeit,
<tb> Diphenylguanidm <SEP> 50, <SEP> 125, <SEP> 156, <SEP> 168 <SEP> "'"
<tb> Di-o-tolylguanidin <SEP> 34, <SEP> 100,150, <SEP> 174 <SEP> , <SEP> ,
<tb> 
 
Die erzielten absoluten Festigkeitswerte sind also wesentlich höher als die   der Verp'leichs-   produkte, welche allgemein angewendet werden. 

**WARNUNG** Ende DESC Feld kannt Anfang CLMS uberlappen**.



   <Desc / Clms Page number 1>
 



  Process to accelerate the vulcanization of Xallchu cards.
 EMI1.1
 
 EMI1.2
 
 EMI1.3
 Represent accelerators which, even with a low sulfur content, give the vulcanizates 20-25% higher tensile strengths. The products of the aforementioned class recognized as new vulcanizers show that there are extremely strong accelerators that are many times better than z. B. Diarylguanidines. The better effectiveness of the vulcanization accelerators according to the present invention results from the following tests:
1st attempt :
 EMI1.4
 
<tb>
<tb> The <SEP> mixture <SEP> consists of <SEP>
<tb> 100-0 <SEP> parts <SEP> rubber.
<tb>



  3-5. <SEP> sulfur,
<tb> 5 # 0 <SEP> ,, <SEP> zinc white,
<tb> 1'0,., <SEP> accelerator.
<tb>



  Accelerator <SEP> 25 ', <SEP> 35', <SEP> 45 '<SEP> at <SEP> 3 <SEP> 1/2 <SEP> Atü.
<tb> Tolylaminoimidazoline <SEP> 204, <SEP> 182, <SEP> 179 <SEP> kg / cm2 <SEP> strength
<tb> Diphenylguanidine <SEP> 170,180, <SEP> 183 <SEP> ,, <SEP> ,,
<tb>
 
 EMI1.5
 Second attempt :
 EMI1.6
 
<tb>
<tb> The <SEP> mixture <SEP> consists of <SEP>
<tb> 100-0 <SEP> parts <SEP> rubber.
<tb>



  25 # 0 <SEP> ,, <SEP> soot,
<tb> 5 # 0 <SEP> ,, <SEP> zinc white.
<tb>



  3-0 <SEP> sulfur,
<tb> 1'0 <SEP> "<SEP> accelerator.
<tb>



  Accelerator <SEP> 10 ', <SEP> 301, <SEP> 601, <SEP> 90' <SEP> at <SEP> 2 # <SEP> Atü.
<tb> Tolylaminoimidazoline <SEP> 108, <SEP> 187, <SEP> 225, <SEP> 204kg / cm3 <SEP> strength,
<tb> Diphenylguanidm <SEP> 50, <SEP> 125, <SEP> 156, <SEP> 168 <SEP> "'"
<tb> Di-o-tolylguanidine <SEP> 34, <SEP> 100,150, <SEP> 174 <SEP>, <SEP>,
<tb>
 
The absolute strength values achieved are therefore significantly higher than those of the comparison products which are generally used.

** WARNING ** End of DESC field may overlap beginning of CLMS **.

 

Claims (1)

PATENT-ANSPRUCH : Verfahren zur Beschleunigung der Vulkanisation von natürlichen oder künstlichen Kautschukarten, dadurch gekennzeichnet, dass man den zu vulkanisierenden Massen Verbindungen der allgemeinen Formel : EMI1.7 EMI1.8 **WARNUNG** Ende CLMS Feld Kannt Anfang DESC uberlappen**. PATENT CLAIM: Process for accelerating the vulcanization of natural or artificial rubber types, characterized in that compounds of the general formula are added to the masses to be vulcanized: EMI1.7 EMI1.8 ** WARNING ** End of CLMS field may overlap beginning of DESC **.
AT122012D 1928-05-15 1929-04-16 Process for accelerating the vulcanization of rubbers. AT122012B (en)