WO2025199676A1 - 负极极片及其制备方法、二次电池及用电装置 - Google Patents

负极极片及其制备方法、二次电池及用电装置

Info

Publication number
WO2025199676A1
WO2025199676A1 PCT/CN2024/083545 CN2024083545W WO2025199676A1 WO 2025199676 A1 WO2025199676 A1 WO 2025199676A1 CN 2024083545 W CN2024083545 W CN 2024083545W WO 2025199676 A1 WO2025199676 A1 WO 2025199676A1
Authority
WO
WIPO (PCT)
Prior art keywords
negative electrode
active material
material layer
current collector
electrode sheet
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/CN2024/083545
Other languages
English (en)
French (fr)
Inventor
赵龙
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ningde Amperex Technology Ltd
Original Assignee
Ningde Amperex Technology Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ningde Amperex Technology Ltd filed Critical Ningde Amperex Technology Ltd
Priority to PCT/CN2024/083545 priority Critical patent/WO2025199676A1/zh
Priority to CN202480004186.XA priority patent/CN120092327A/zh
Publication of WO2025199676A1 publication Critical patent/WO2025199676A1/zh
Anticipated expiration legal-status Critical
Pending legal-status Critical Current

Abstract

一种负极极片及其制备方法、二次电池及用电装置,包括负极集流体、第一活性物质层和第二活性物质层,沿负极集流体的厚度方向,负极集流体具有相对设置的第一表面和第二表面,第一活性物质层设置于第一表面,第二活性物质层设置于第二表面。沿负极极片的长度方向,第一活性物质层的一端为第一端部,第二表面具有第一空集流体区。沿负极极片的厚度方向观察,第一端部的投影与第一空集流体区至少部分重叠。第二表面对应的第一端部处无活性物质层,可使得负极极片在第一端部处的整体厚度减小,在冷压辊压负极极片时,可有效减少负极极片出现过压,从而减少负极集流体出现损伤断裂。

Description

负极极片及其制备方法、二次电池及用电装置 技术领域
本申请涉及电池技术领域,特别是涉及一种负极极片及其制备方法、二次电池及用电装置。
背景技术
锂离子电池具有能量密度高,循环寿命长,便携易带等优点被广泛应用于各种储能领域,随着近些年来消费类锂离子电池不断迭代开发,市场对电池的能量密度要求越来越高。
提升能量密度以及增强快充性能是锂离子电池行业的目标之一,增加极片活性物质的负载量,不但能提升能量密度,还能达到降低成本的目的。为此开发出了双层涂布技术,但是双层涂布,在冷压辊压时,因两面均存在活性物质层,非常容易出现过压,造成极片的集流体出现损伤,导致在极片后续加工过程中易出现断带。为保证后续加工,多数情况下是降低压实密度,这样导致能量密度损失,失去了双层涂布提高能量密度的意义。
发明内容
本申请的目的在于提供一种负极极片及其制备方法、二次电池及用电装置,旨在改善集流体易过压损坏的技术问题。
根据本申请的第一方面,提供一种负极极片,包括负极集流体、第一活性物质层和第二活性物质层,沿负极集流体的厚度方向,负极集流体具有相对设置的第一表面和第二表面,第一活性物质层设置于第一表面,第二活性物质层设置于第二表面。沿负极极片的长度方向,第一活性物质层的一端为第一端部,第二表面具有第一空集流体区。沿负极极片的厚度方向观察,第一端部的投影与第一空集流体区至少部分重叠,沿负极极片的长度方向,第一活性物质层还包括与第一端部相对设置的 第二端部,第二表面还具有第二空集流体区。沿负极极片的厚度方向观察,第二端部的投影与第二空集流体区至少部分重叠。
上述技术方案中,第一端部的投影与第一空集流体区至少部分重叠,第二表面与第一端部对应的地方无活性物质层,第二表面与第二端部对应的地方无活性物质层,即在负极极片的第一端部和第二端部,负极集流体两侧负极活性物质层均错位,在负极极片长度方向上,第一活性物质层长度长于第二活性物质层,且第一活性物质层在第一集流体上的投影长度完全覆盖第二活性物质层在第一集流体上的长度,如此,可使得负极极片在第一端部处的整体厚度减小,在冷压辊压负极极片时,可有效减少负极极片出现过压,从而减少负极集流体出现损伤断裂,相对于传统的方案,本申请中,无需降低第一活性物质层和/或第二活性物质层的压实密度,可保证负极极片具有较高的能量密度。本申请所述空集流体区指集流体的某一表面上未设置活性物质层的区域。
在一些优选的实施方式中,沿负极极片的厚度方向观察,沿负极极片的长度方向,第一端部与第一空箔区重叠的长度为L1mm,3mm≤L1≤100mm。通过将第一活性物质层的第一端部与第二活性物质层设置错位长度为3mm及以上,可以使得负极极片在冷压辊压过程中,避免端部对齐而导致端部的局部厚度增加,从而减少负极集流体在各活性物质层的端部处因受力过大而破损,同时降低工艺控制难度;将第一活性物质层的第一端部与第二活性物质层设置错位长度为100mm及以下可以避免二次电池能量密度的过分损失。值得注意的是,上述L1的范围选择的技术效果为本申请优选技术效果,只要第一活性物质层的第一端部与第二活性物质层错位设置,就可实现本申请的基础的减小负极极片过压的技术效果,后文优选实施方式同理。
在一些优选的实施方式中,沿负极极片的厚度方向观察,沿负极极片的长度方向,第二端部与第二空箔区重叠的长度为L2mm,3mm≤L2≤100mm。通过将第一活性物质层的第二端部与第二活性物质层设置错位长度为3mm及以上,可以使得负极极片在冷压辊压过程中,避免端部对齐而导致端部的局部厚度增加,从而减少负极集流体在各活性物质层的端部处因受力过大而破损,同时降低工艺控制难度;将第一 活性物质层的第二端部与第二活性物质层设置错位长度为100mm及以下可以避免二次电池能量密度的过分损失。
在一些优选的实施方式中,第一活性物质层包括第一活性材料,第二活性物质层包括第二活性材料,第二活性材料的克容量大于第一活性材料的克容量。由于第二表面与第一端部和第二端部对应的地方均无活性物质层,即第二活性物质层长度较第一活性物质层长度段,使第二活性材料的克容量大于第一活性材料的克容量,可以弥补容量损失,提高二次电池容量。
在一些优选的实施方式中,第一活性材料的克容量为345mAh/g~355mAh/g,第二活性材料的克容量为358mAh/g~365mAh/g。
第二方面,本申请还提出了一种二次电池,包括壳体以及电极组件,电极组件收容于壳体内,电极组件包括正极极片、隔离膜以及如上述第一方面任一实施例的负极极片。正极极片、隔离膜以及负极极片层叠并卷绕设置,第一表面背离卷绕中心设置,第二表面面向卷绕中心设置。
在一些优选的实施方式中,正极极片包括正极集流体、第三活性物质层和第四活性物质层,第三活性物质层设置于正极集流体的面向第二活性物质层的表面,第四活性物质层设置于正极集流体的背离第二活性物质层的表面。正极集流体电连接有正极极耳,第二活性物质层上开设有第一避让槽。在正极集流体的位于正极极耳的位置,沿正极集流体的厚度方向观察,正极极耳的投影落入第一避让槽中。由于对应的负极极片处具有避让正极极耳的第一避让槽,因此可减少连接正极极耳后导致正极极片厚度增加而影响电池能量密度的问题。由于负极极片的第二活性物质开设第一避让槽,为了防止析锂,可以在正极极耳区域贴保护胶层,保护胶层的投影面积完全覆盖第一避让槽。
在一些优选的实施方式中,负极集流体电连接有负极极耳,第三活性物质上开设有第二避让槽。在负极集流体的位于负极极耳的位置,沿负极集流体的厚度方向观察,负极极耳的投影落入第二避让槽中,可减少连接负极极片后导致正极极片厚度增加的问题,减少电池的能量密度损失。同时,在正极极片对应负极极耳的位置开设置第二避让槽,减少了正极活性物质层的余量,从而保证负极极片具有足够的余量来嵌入正 极脱出的锂离子,从减少电池析锂。
在一些优选的实施方式中,第一端部和第一空箔区靠近卷绕中心设置,沿负极极片的厚度方向观察,第一端部与第一空箔区重叠的长度为L1mm,60mm≤L1≤100mm。第一活性物质层还具有远离卷绕中心设置的第二端部,第二表面具有远离卷绕中心的第二空箔区,沿负极极片的厚度方向观察,第二端部与第二空箔区重叠的长度为L2mm,3mm≤L2≤8mm。
第三方面,本申请还提供一种用电装置,包括以上第二方面任一实施例的二次电池。
第四方面,本申请还提出了一种制备如上述第一方面任意实施例的负极极片的方法,包括:
提供负极集流体,沿负极集流体厚度方向,负极集流体具有相对设置的第一表面和第二表面;
在第一表面设置连续的第一活性物质层;
沿负极集流体的长度方向,在第二表面设置若干间隔排列的第二活性物质层,相邻的两个第二活性物质层之间形成间隔区域;
在间隔区域,对负极集流体以及第一活性物质层进行裁剪,以形成多个负极极片;其中,于间隔区域,第一表面至少形成一个负极极片的第一空集流体区。
本申请实施例的额外层面及优点将部分地在后续说明中描述、显示、或是经由本申请实施例的实施而阐释。
附图说明
一个或多个实施例通过与之对应的附图进行示例性说明,这些示例性说明并不构成对实施例的限定,附图中具有相同参考数字标号的元件表示为类似的元件,除非特别申明,附图中的尺寸不构成比例限制。
图1示出了本申请一些实施例的负极极片的结构示意图;
图2示出了本申请一些实施例的电极组件的卷绕结构示意图;
图3示出了本申请一些实施例的负极极片的结构示意图;
图4示出了本申请一些实施例的二次电池的结构示意图;
图5为图2中A处的局部放大图;
图6为图2中B处的局部放大图;
图7为图2中C处的局部放大图;
图8为负极极片卷的结构示意图;
图9负极极片的裁剪制备示意图。
附图标记说明:
10、负极极片;11、负极集流体;11a、第一表面;11b、第二表面;
111、第一空集流体区;112、第二空集流体区;12、第一活性物质层;121、第一端部;122、第二端部;13、第二活性物质层;
1000、二次电池;
100、壳体;
200、电极组件;210、正极极片;211、正极集流体;212、第三活
性物质层;213、第四活性物质层;2121、第二避让槽;220、负极极片卷;11、负极集流体;12、第一活性物质层;13、第二活性物质层;131、第一避让槽;230、隔离膜;240、正极极耳;250、负极极耳;260、间隔区域;
X、第二方向;Y、第三方向;Z、第一方向。
具体实施方式
为使本申请实施例的目的、技术方案和优点更加清楚,下面将结合本申请实施例中的附图,对本申请实施例中的技术方案进行清楚地描述,显然,所描述的实施例是本申请一部分实施例,而不是全部的实施例。
在本申请中提及“实施例”意味着,结合实施例描述的特定特征、结构或特性可以包含在本申请的至少一个实施例中。在说明书中的各个位置出现该短语并不一定均是指相同的实施例,也不是与其它实施例互斥的独立的或备选的实施例。
在本申请实施例的描述中,术语“和/或”仅仅是一种描述关联对象的关联关系,表示可以存在三种关系,例如A和/或B,可以表示:单独存在A,同时存在A和B,单独存在B这三种情况。另外,本文中字符“/”,一般表示前后关联对象是一种“或”的关系。
下面所描述的本申请不同实施例中所涉及的技术特征只要彼此之 间未构成冲突就可以相互结合。
第一方面,本申请的提出了一种负极极片,请参照图1,该负极极片10包括负极集流体11、第一活性物质层12以及第二活性物质层13,其中,第一活性物质层12和第二活性物质层13分别设置于集流体厚度方向(第一方向Z)的两个表面。
对于上述负极集流体11,负极集流体11是负极极片10中的导电部分,能够将活性物质产生的电子传递到外部电路。负极集流体11通常具有较高的机械强度,能够提高负极极片10的整体强度,减少在电池充放电过程中负极极片10发生变形或破裂。例如,负极集流体11可采用强度较高的金属材质,具体的可采用整体扁平且呈条状结构的铜箔、镍箔或者聚合物铜箔(铜箔表面设置有聚乙烯、聚丙烯或聚酰胺等高分子聚合物)等。负极集流体11为活性物质提供了支撑和固定的平台,使活性物质能够均匀地分布在负极集流体11上,保证负极极片10的结构稳定性。
对于上述第一活性物质层12和第二活性物质层13,请参照图1,沿负极集流体11的厚度方向(第一方向Z),负极集流体11包括相对设置的第一表面11a和第二表面11b,第一活性物质层12可设置于第一表面11a,第二活性物质层13可设置于第二表面11b。第一活性物质层12和第二活性物质层13在电池充放电过程中参与一些列的电化学反应,从而实现电能和化学能之间的转换。以锂离子电池为例,在电池充电过程中,锂离子从正极脱出,通过电解液迁移到第一活性物质层12和/或第二活性物质层13中。而在电池放电过程中,锂离子从第一活性物质层12和/或第二活性物质层13中脱出,通过电解液回到正极,完成电池的充放电循环。
其中,第一活性物质层12包括第一活性材料、导电剂以及粘接剂等,此类材料混合后搅拌均匀并涂覆于负极集流体11的表面,从而得到第一活性物质层12。其中,第一活性材料可选自石墨、软碳、硬碳、碳纤维、单质硅、硅氧化合物、硅合金中的一种或多种;第二活性物质层13同理。
本申请的实施例中,采用双层活性物质层的负极极片10可有效提 高电池的能量密度,在第一活性物质层12和/或第二活性物质层13的端部处(负极极片11长度方向的两端,也即图1中第二方向X的两端),易出现凸起结构,尤其当第一活性物质层12与第二活性物质层13的端部重叠时,其凸起结构也可能重叠,导致负极极片10在活性物质层的各端部处出现厚度增大,在冷压辊压负极极片10时,很容易导致负极集流体11过压,造成负极集流体11损伤,以致于负极极片10在后续加工过程中出现断裂。
为缓解上述问题,沿负极极片10的长度方向(第二方向X),第一活性物质层12的一端为第一端部121,第二表面11b具有第一空集流体区111,沿负极极片10的厚度方向(第一方向Z)观察,第一端部121的投影与第一空集流体区111至少部分重叠。负极极片10的长度方向(第二方向X),第一活性物质层12还包括与第一端部121相对设置的第二端部122,第二表面11b还具有与第一空集流体区111相对设置的第二空集流体区112。沿负极极片10的厚度方向(第一方向Z)观察,第二端部122的投影与第二空集流体区112至少部分重叠。第二表面11b对应的第一端部121处无活性物质层,即在负极极片10的第一端部121,负极集流体11两侧的活性物质层错位,第二表面11b对应的第二端部122处无活性物质层,即在负极极片10的第二端部122,负极集流体11两侧的活性物质层错位,可使得负极极,片10在第一端部121和第二端部122处的整体厚度减小,在冷压辊压负极极片10时,可有效减少负极极片10出现过压,从而减少负极集流体11出现损伤断裂;同时,无需降低第一活性物质层12和/或第二活性物质层13的压实密度,以保证负极极片10具有较高的能量密度。其中,本申请所述空集流体区指集流体的某一表面上未设置活性物质层的区域。
请参照图1,在一些实施例中,沿负极极片10的厚度方向(第一方向Z)观察,沿负极极片10的长度方向(第二方向X),第一端部121与第一空箔区重叠的长度为L1mm,3mm≤L1≤100mm。通过将第一活性物质层12的第一端部121与第二活性物质层13设置错位长度为3mm及以上,可以使得负极极片10在冷压辊压过程中,避免端部对齐而导致端部的局部厚度增加,从而减少负极集流体11在各活性物质层的端 部处因受力过大而破损。同时降低工艺控制难度;将第一活性物质层12的第一端部121与第二活性物质层13设置错位长度为100mm及以下可以减少二次电池能量密度的过分损失。值得注意的是,上述L1的范围选择的技术效果为本申请优选技术效果,只要第一活性物质层12的第一端部121与第二活性物质层13错位设置,就可实现本申请的基础的减小负极极片10过压的技术效果,后文优选实施方式同理。
请参照图1,沿负极极片10的厚度方向(第一方向Z)观察,沿负极极片10的长度方向(第二方向Y),第二端部122与第二空集流体区112重叠的长度为L2mm,3mm≤L2≤100mm。通过将第一活性物质层12的第二端部122与第二活性物质层13设置错位长度为3mm及以上,可以使得负极极片10在冷压辊压过程中,避免端部对齐而导致端部的局部厚度增加,从而减少负极集流体11在各活性物质层的端部处因受力过大而破损。同时降低工艺控制难度;将第一活性物质层12的第二端部122与第二活性物质层13设置错位长度为100mm及以下可以避免二次电池能量密度的过分损失。
例如,当上述的负极极片10应用在叠片型电极组件200中时,L1和L2的取值可以较小,例如3mm≤L1≤8mm、3mm≤L2≤8mm。由于第一活性物质层12和第二活性物质层13错位长度(也即第一端部121与第一空集流体区111的重叠长度)在3mm时就能够有效改善在辊压时负极集流体11容易被压破损的问题,为了降低加工难度,可以适当增加第一端部121与第一空集流体区111的重叠长度。而为了保证负极极片10能够具有较高的能量密度,重叠长度不宜过长,因此可设置为8mm以下,可在减少负极集流体11被压破损的同时,保证负极极片10具有较高的能量密度。
当上述的负极极片10应用在卷绕型电极组件200中时,第一端部121和第二端部122二者中靠近卷绕中心的一者的长度可以取较大值,而远离卷绕中心的一者的长度可以取较小值。作为一种示例,请参照图2,第一端部121靠近卷绕中心,其长度L1满足60mm≤L1≤100mm,在靠近电极组件200的卷绕中心处,由于负极极片10面向卷绕中心的内侧没有对应的正极极片210,位于负极极片10的内侧上的活性物质材料 无法参与电化学反应,因此,为了降低电极组件200的重量,以及提升电极组件200的能量密度,负极极片10的卷绕首圈仅一面设置有活性物质层,内侧通常设置成空集流体区,其长度可设置为60mm至100mm。
而在靠近电极组件200的卷绕中心处,负极极片10背离卷绕中心的外侧存在对应的正极极片210,在负极极片10的外侧设置有活性物质层可以与正极极片210上的活性物质层参与电化学反应,也即第一端部121与第一空集流体区111可以至少部分重叠,因此其重叠长度可设置60mm至100mm。
第二端部122远离卷绕中心,其长度L2满足3mm≤L2≤8mm,在远离卷绕中心处,负极极片10面向卷绕中心的内侧或背离卷绕中心的外侧都可能存在对应的正极极片210,因此负极极片10在远离卷绕中心一端的空集流体区不宜过大。第二端部122与第二空集流体区112的3mm重叠长度即可有效改善在冷压辊压时负极集流体11容易被压破损的问题,为了降低加工难度,可以适当增加第一端部121与第一空集流体区111的重叠长度。而为了保证负极极片10能够具有较高的能量密度,重叠长度不宜过长,因此可设置为8mm以下,可在减少负极集流体11被压破损的同时,保证负极极片10具有较高的能量密度。其中,当第二端部122靠近卷绕中心时,其长度L2也可满足60mm≤L2≤100mm。
在一些实施例中,第一活性物质层12包括第一活性材料,第二活性物质层13包括第二活性材料,第二活性材料的克容量大于所述第一活性材料的克容量。第二活性物质层13采用克容量更大的第二活性材料,可提高电池的能量密度。例如,第一活性材料的克容量为345mAh/g~355mAh/g,第二活性材料的克容量为358mAh/g~365mAh/g,其中第一活性材料和第二活性材料均可采用上述石墨、软碳、硬碳或碳纤维等,以石墨为例,不同石墨的克容量可能会存在差异,例如高结晶度的石墨通常具有更高的克容量,因为其晶体结构更有序,有利于锂离子的嵌入和脱出,较小的晶粒尺寸也可以提供更多的活性表面积,促进电化学反应,从而提高克容量;此外,石墨的纯度和表面形貌也会对克容量产生影响,纯度高的石墨通常具有更好的电化学性能,而经过表面处理或改性的石墨可以改善其与电解液的润湿性和反应活性,从而提高 克容量。
在一些实施例中,第一活性物质层12可以为单层涂覆结构,也可以是双层或者多层涂覆结构。作为一种示例,请参照图3,第一活性物质层12为双层涂覆结构,第一活性物质层12包括第一涂层12a和第二涂层12b,第二涂层12b设置在第一涂层12a与负极集流体11之间。本申请中通过设置动力学性能不同的第一涂层12a和第二涂层12b的结构,既可以提升第一活性物质层12的动力学性能,也可以使得第一活性物质层12具有较高的能量密度。可选的,第一涂层12a与第二涂层12b也可进行错位堆叠,可以有效减少第一活性物质层12的端部的厚度过厚的问题,降低在冷压辊压的过程中,负极集流体11出现断裂失效的风险。第二活性物质层13也可与第一活性物质层12类似设置。
第二方面,本申请还提出了一种二次电池1000,请参照图2和图4,该二次电池1000包括壳体100以及电极组件200,电极组件200收容于壳体100内。其中,电极组件200包括正极极片210、隔离膜230以及负极极片10,正极极片210、隔离膜230以及负极极片10层叠并卷绕设置。
其中,负极集流体11的第一表面11a背离卷绕中心设置,第二表面11b面向卷绕中心设置。在负极极片10卷绕后,第一表面11a背离卷绕中心,为负极长面,因此可设置长度尺寸更大的第一活性物质层12;第二表面11b面向卷绕中心,为负极短面,因此采用长度尺寸更小的第二活性物质层13。
请参照图2、图4和图5,正极极片210包括正极集流体211、第三活性物质层212和第四活性物质层213,正极集流体211作为正极极片210的导电基材,其可采用整体扁平且呈条状结构的铝箔,第三活性物质层212和第四活性物质层213分别设置于正极集流体211厚度方向的两个表面。例如,第三活性物质层212设置于正极集流体211的面向第二活性物质层13的表面,第四活性物质层213设置于正极集流体211的背离第二活性物质层13的表面。正极集流体211电连接有正极极耳240,可电连接方式可为焊接、卡接或导电胶粘接等。
其中,第三活性物质层212以及第四活性物质层213包括正极活性 材料、导电剂以及粘接剂等,上述各材料组分混合后搅拌均匀并涂覆于正极集流体211厚度方向的两个表面,从而得到第三活性物质层212和第四活性物质层213。正极活性材料可选自镍钴锰酸锂、钴酸锂、磷酸铁锂、镍钴锰酸锂、锰酸锂、磷酸锰铁锂、无钴材料中的一种或多种。
请参照图6,第二活性物质层13上开设有第一避让槽131,在正极集流体211的位于正极极耳240的位置,沿正极集流体211的厚度方向(第一方向Z)观察,正极极耳240的投影落入第一避让槽131中,即第一避让槽131完全覆盖正极极耳240。例如,在第三活性物质层212开设有第一极耳槽(图中未标示),正极极耳240于第一极耳槽内与正极集流体211电连接,在正极极片210、隔离膜230以及负极极片10层叠并卷绕时,正极极耳240即使凸出第一极耳槽,由于对应的负极极片10处具有避让正极极耳240的第一避让槽131,因此可减少连接正极极耳240后导致正极极片210厚度增加而影响电池能量密度的问题。
请参照图7,负极集流体11电连接有负极极耳250,负极极片10也可通过焊接、卡接或导电胶粘接等方式与负极集流体11直接电连接。正极极片210的第三活性物质上开设有第二避让槽2121,在负极集流体11的位于负极极耳250的位置,沿负极集流体11的厚度方向(第一方向Z)观察,负极极耳250的投影落入第二避让槽2121中,即第二避让槽2121完全覆盖负极极耳250,可减少连接负极极片10后导致正极极片210厚度增加的问题,减少电池的能量密度损失。同时,在正极极片210对应负极极片10的位置开设置第二避让槽2121,减少了正极活性物质层的余量,从而保证负极极片10具有足够的余量来嵌入正极脱出的锂离子,从减少电池析锂。
第一端部121和第一空集流体区111靠近卷绕中心设置,沿负极极片10的厚度方向(第一方向Z)观察,第一端部121与第一空集流体区111重叠的长度为L1mm,60mm≤L1≤100mm;在电极组件200的卷绕中心处,由于负极极片10的内侧没有对应的正极极片210,位于负极极片10的内侧上的活性物质材料无法参与电化学反应,因此,为了降低电极组件200的重量,以及提升电极组件200的能量密度,负极极片10中靠近卷绕中心的端部的内侧通常设置成空集流体区,即不涂覆活性物质 层,该空集流体区在电极组件200的内圈卷绕,其长度可为60mm至100mm。而在靠近电极组件200的卷绕中心处,负极极片10背离卷绕中心的外侧有对应的正极极片210,因此,在负极极片10的外侧设置有活性物质层可以与正极极片210上的活性物质层参与电化学反应,也即在第一端部121构成了负极集流体11的两个表面上的活性物质层的错位设置。
第一活性物质层12还具有远离所述卷绕中心设置的第二端部122,第二表面11b具有远离卷绕中心的第二空集流体区112,沿负极极片10的厚度方向(第一方向Z)观察,第二端部122与所述第二空箔区重叠的长度为L2mm,3mm≤L2≤8mm。第一活性物质层12和第二活性物质层13错位长度在3mm时即可有效改善在辊压时负极集流体11容易被压破损的问题,为了降低加工难度,可以适当增加第一活性物质层12和第二活性物质层13的错位长度。而为了保证负极极片10能够具有较高的能量密度,第一活性物质层12和第二活性物质层13的错位长度不宜设置过长,因此可设置为8mm以下。
第三方面,本申请提出一种用电装置,包括上述第一方面任一实施例的二次电池1000。
第四方面,本申请还提出了一种负极极片10的制备方法,请参照图8和图9,其中图8示出了负极极片卷220的结构,图9示出了裁剪负极极片卷220以形成负极极片10的结构,所述方法包括:
提供负极集流体11,沿负极集流体11厚度方向,负极集流体11具有相对设置的第一表面11a和第二表面11b;
在第一表面11a设置连续的第一活性物质层12;
沿负极集流体11的长度方向(第二方向X),在第二表面11b设置若干间隔排列的第二活性物质层13,相邻的两个第二活性物质层13之间形成间隔区域260;
在间隔区域260,对负极集流体11以及第一活性物质层12进行裁剪,以形成多个负极极片10;其中,于间隔区域260,第一表面11a至少形成一个负极极片10的第一空集流体区111。可以理解的是,在间隔 区域260,第一表面11a还可能形成另一个负极极片10的第二空集流体区112。
采用上述方法制备的负极极片10,在冷压辊压负极极片10时,可有效减少负极极片10出现过压,从而减少负极集流体11出现损伤断裂;相对于传统的方案,无需降低第一活性物质层12和/或第二活性物质层13的压实密度,可保证负极极片10具有较高的能量密度。
本申请的实施例中,对负极极片进行冷压测试:
实施例1
为便于理解本申请的技术构思和技术效果,下面以锂离子电池为例进行实验说明。
实验一:[负极极片大卷的制备]
实施例1
将人造石墨(克容量=350mAh/g)、羧甲基纤维素(CMC,重均分子量9.0×105)、粘结剂丁苯橡胶(SBR,重均分子量为5×106)、按照质量比97.8:1.2:1进行混合,然后加入去离子水作为溶剂,在真空搅拌机作用下搅拌至固含量为50wt%且体系均匀的第一浆料。
将人造石墨(克容量=362Ah/g,温度系数=97.5%)、羧甲基纤维素(CMC,重均分子量9.0×105)、粘结剂丁苯橡胶(SBR,重均分子量为5×106)、按照质量比97.5:1.2:1.3进行混合,然后加入去离子水作为溶剂,在真空搅拌机作用下搅拌至固含量为50wt%且体系均匀的第二浆料。
通过单腔体挤压涂布模头将第一浆料均匀涂覆在厚度为8μm的负极集流体铜箔(抗拉强度=500MPa)厚度方向的一个表面上,90℃条件下烘干,得到涂覆有第一活性物质层的负极极片大卷;将第二浆料均匀涂覆在负极集流体铜箔厚度方向的另一个表面,90℃条件下烘干,得到涂覆有第一活性物质层和第二活性物质层的负极极片大卷,冷压前第一活性物质层和第二活性物质层的厚度为110μm。将负极极片在290℃下烘烤处理10h后,在湿度<5%的环境下降温至室温。
其中,负极集流体两侧的活性物质层在负极集流体展开时的长度方向上呈两端均错位设置结构,具体的,第一端部长度为60mm(第一端部与第一空集流体区重叠的长度L1=60mm),第二端部长度3mm(第二端部与第二空集流体区重叠的长度L2=3mm)。
实施例2至13:除了第一单侧涂覆部的长度L1和/或第二单侧涂覆部的长度L2的长度不同之外,其余参数与实施例1相同,具体请参阅下表1。
对比例1中,采用的是集流体两侧的活性物质层对齐,即L1=0mm,L2=0mm。
断带率测试方法:取1000米左右收卷涂布后的负极极片,在冷压机中进行过辊冷压,极片压实密度设置为1.7g/cm3,冷压前总米数Y,冷压过程中因断带造成损耗的米数为Y’,则冷压断带率=Y’/Y×100%。
表1
根据上述表1,结合对比例1以及实施例1至8可知,负极极片上的活性物质层两端呈错位设置时,可有效降低负极极片在生产大卷的过 程中的断带率,提升大卷生产的连续性和产品质量。在L1相同的情况下,实施例1、实施例3、实施例4的断带率明显低于施例2,可见将错位长度设置在3mm以上可以进一步降低断带率,实施例5-8的断带率相比实施例1、实施例3、实施例4并无进一步提升,但实施例1、实施例3、实施例4中,错位长度更短,对能量密度影响更小,因此,本申请中,优选错位长度为3mm至8mm,可进一步降低负极极片在生产中的断带率并兼顾能量密度。值得注意的是,对于负极极片的生产过程中的断带而言,L1和L2对断带率的影响规律是一样的。
实验二:[锂离子电池的热压通过率测试]
实施例14
<负极极片的制备>
通过裁切实施例1中的负极极片大卷,得到单面涂覆厚度为90μm,宽×长为76mm×860mm的负极极片,在负极极片上通过激光开出12mm×35mm负极极耳槽位,在负极极耳槽位中焊接厚度为110μm,宽×长为8mm×55mm的负极极耳。
<正极极片的制备>
将正极活性材料磷酸铁锂、正极导电剂乙炔黑、正极粘结剂聚偏二氟乙烯(PVDF,重均分子量为5×105)按照质量比94:3:3进行混合,加入N-甲基吡咯烷酮(NMP)作为溶剂,在真空搅拌机作用下搅拌至固含量为75wt%且体系均匀的正极浆料。将正极浆料均匀涂布在厚度为6um的正极集流体铝箔的一个表面上,90℃条件下烘干,得到单面涂布正极活性物质层(厚度80μm)的正极极片。之后,在该铝箔的另一个表面上重复以上步骤,得到双面涂布正极活性物质层的正极极片。再经冷压、分切,在正极极片上通过激光开出10mm×35mm正极极耳槽位,在正极极耳槽位中焊接厚度为116μm,宽×长为5mm×55mm的正极极耳得到规格为74mm×851mm正极极片待用。
<隔膜>以厚度为8μm的聚乙烯(PE)多孔薄膜作为隔膜。
<电解液的制备>
在干燥氩气气氛中,将碳酸乙烯酯、碳酸甲乙酯和碳酸二乙酯以质量比30:50:20混合得到有机溶液,然后向有机溶剂中加入锂盐六氟磷酸锂溶解并混合均匀,得到锂盐的浓度为1.15mol/L的电解液。
<锂离子电池的制备>
将上述制备得到的隔膜、正极极片、隔膜、负极极片按顺序叠好,卷绕得到电极组件,电极组件中负极极片的第一活性物质层背离卷绕中心面,第二活性物质层面向卷绕中心面,第一端部与第一空箔区靠近卷绕中心设置(即为负极极片卷绕起始端),对电极组件进行热压,压力5MPa,温度65℃,保压时间10s。将电极组件放入外包装铝塑膜中,在80℃下脱去水分后,注入电解液并封装,经过化成、脱气、整形等工艺流程得到锂离子电池。
实施例15:在实施例14的基础上,在负极极片第二活性物质层上用激光开设14mm×40mm的第一避让槽,并在正极极耳区域贴20mm×50mm的绿胶。
实施例15:在实施例14的基础上,在负极极片第二活性物质层上用激光开设14mm×40mm的第一避让槽,并在正极极耳区域贴20mm×50mm的绿胶。
实施例16:在实施例15的基础上,在与负极极耳相对的正极极片活性物质层上开设用激光开设14mm×40mm的第二避让槽。
对比例2:通过裁切对比例1中的负极极片大卷,得到适合制作锂离子电池的负极极片。其余参数与实施例14中的制备参数相同,此处不再赘述。
选择实施例14-16和对比例2制备的电池各10个,通过千分尺测量各电池的最大厚度,并求平均值,然后进行热压测试实验(热压条件:热压压力0.25MPa,温度65℃,时间4s),实验完成后,将锂离子电池拆开记录负极集流体破损的数量,如下表2所示。
表2
通过对比例2和实施例14-16可知,锂离子电池中采用活性物质层的两端均错位设置的负极极片可以有效提升锂离子电池在热压实验中的通过率,从而提升锂离子电池的安全性能,开设第一避让槽和第二避让槽可以在一定层度降低电池最大厚度,提高能量密度。
以上所述仅为本申请的实施例,并非因此限制本申请的专利范围,凡是利用本申请说明书及附图内容所作的等效结构或等效流程变换,或直接或间接运用在其他相关的技术领域,均同理包括在本申请的专利保护范围内。

Claims (11)

  1. 一种负极极片,包括负极集流体、第一活性物质层和第二活性物质层,沿所述负极集流体的厚度方向,所述负极集流体具有相对设置的第一表面和第二表面,所述第一活性物质层设置于所述第一表面,所述第二活性物质层设置于所述第二表面,其特征在于:
    沿所述负极极片的长度方向,所述第一活性物质层的一端为第一端部,所述第二表面具有第一空集流体区;
    沿所述负极极片的厚度方向观察,所述第一端部的投影与所述第一空集流体区至少部分重叠;
    沿所述负极极片的长度方向,所述第一活性物质层还包括与所述第一端部相对设置的第二端部,所述第二表面还具有第二空集流体区;
    沿所述负极极片的厚度方向观察,所述第二端部的投影与所述第二空集流体区至少部分重叠。
  2. 根据权利要求1所述的负极极片,其特征在于,沿所述负极极片的厚度方向观察,沿所述负极极片的长度方向,所述第一端部与所述第一空箔区重叠的长度为L1mm,3mm≤L1≤100mm。
  3. 根据权利要求1所述的负极极片,其特征在于,沿所述负极极片的厚度方向观察,沿所述负极极片的长度方向,所述第二端部与所述第二空箔区重叠的长度为L2mm,3mm≤L2≤100mm。
  4. 根据权利要求1-3任一项所述的负极极片,其特征在于,所述第一活性物质层包括第一活性材料,所述第二活性物质层包括第二活性材料,所述第二活性材料的克容量大于所述第一活性材料的克容量。
  5. 根据权利要求4所述的负极极片,其特征在于,所述第一活性材料的克容量为345mAh/g~355mAh/g,所述第二活性材料的克容量为358mAh/g~365mAh/g。
  6. 一种二次电池,包括壳体以及电极组件,所述电极组件收容于所述壳体内,其特征在于,所述电极组件包括正极极片、隔离膜以及如权利要求1至5中任一项所述的负极极片;
    所述正极极片、隔离膜以及负极极片层叠并卷绕设置,所述第一表面背离卷绕中心设置,所述第二表面面向卷绕中心设置。
  7. 根据权利要求6所述的二次电池,其特征在于,所述正极极片包括正极集流体、第三活性物质层和第四活性物质层,所述第三活性物质层设置于所述正极集流体的面向所述第二活性物质层的表面,所述第四活性物质层设置于所述正极集流体的背离所述第二活性物质层的表面;
    所述正极集流体电连接有正极极耳,所述第二活性物质层上开设有第一避让槽;
    沿所述正极集流体的厚度方向观察,所述正极极耳的投影落入所述第一避让槽中。
  8. 根据权利要求7所述的二次电池,其特征在于,所述负极集流体电连接有负极极耳,所述第三活性物质上开设有第二避让槽;
    沿所述负极集流体的厚度方向观察,所述负极极耳的投影落入所述第二避让槽中。
  9. 根据权利要求6-8任一项所述的二次电池,其特征在于,所述第一端部和所述第一空箔区靠近所述卷绕中心设置,沿所述负极极片的厚度方向观察,所述第一端部与所述第一空箔区重叠的长度为L1mm,60mm≤L1≤100mm;
    所述第一活性物质层还具有远离所述卷绕中心设置的第二端部,所述第二表面具有远离所述卷绕中心的第二空箔区,沿所述负极极片的厚度方向观察,所述第二端部与所述第二空箔区重叠的长度为L2mm,3mm≤L2≤8mm。
  10. 一种用电装置,其特征在于,包括权利要求6-9任一项所述的二次电池。
  11. 一种制备如权利要求1至5中任一项所述的负极极片的方法,其特征在于,包括:
    提供负极集流体,沿所述负极集流体厚度方向,所述负极集流体具有相对设置的第一表面和第二表面;
    在所述第一表面设置连续的第一活性物质层;
    沿所述负极集流体的长度方向,在所述第二表面设置若干间隔排列的第二活性物质层,相邻的两个第二活性物质层之间形成间隔区域;
    在所述间隔区域,对所述负极集流体以及第一活性物质层进行裁剪,以形成多个负极极片;其中,于所述间隔区域,所述第一表面至少形成一个所述负极极片的所述第一空集流体区。
PCT/CN2024/083545 2024-03-25 2024-03-25 负极极片及其制备方法、二次电池及用电装置 Pending WO2025199676A1 (zh)