WO2025126879A1 - 基板処理方法、基板処理装置、および基板処理システム - Google Patents

基板処理方法、基板処理装置、および基板処理システム Download PDF

Info

Publication number
WO2025126879A1
WO2025126879A1 PCT/JP2024/042503 JP2024042503W WO2025126879A1 WO 2025126879 A1 WO2025126879 A1 WO 2025126879A1 JP 2024042503 W JP2024042503 W JP 2024042503W WO 2025126879 A1 WO2025126879 A1 WO 2025126879A1
Authority
WO
WIPO (PCT)
Prior art keywords
substrate
silicon
containing film
stress
substrate processing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
PCT/JP2024/042503
Other languages
English (en)
French (fr)
Japanese (ja)
Inventor
健次 大内
孝広 宮原
晋 山内
嵩大 荻野
好太 梅澤
勝利 石井
亮太 井福
佳優 渡部
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Tokyo Electron Ltd
Original Assignee
Tokyo Electron Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Tokyo Electron Ltd filed Critical Tokyo Electron Ltd
Priority to KR1020267021301A priority Critical patent/KR20260121466A/ko
Publication of WO2025126879A1 publication Critical patent/WO2025126879A1/ja
Anticipated expiration legal-status Critical
Pending legal-status Critical Current

Links

Images

Classifications

    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/24—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials using chemical vapour deposition [CVD]
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/24—Deposition of silicon only
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/40—Oxides
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/22—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the deposition of inorganic material, other than metallic material
    • C23C16/30—Deposition of compounds, mixtures or solid solutions, e.g. borides, carbides, nitrides
    • C23C16/40—Oxides
    • C23C16/401—Oxides containing silicon
    • C23C16/402—Silicon dioxide
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/44—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating
    • C23C16/46—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating characterised by the method used for heating the substrate
    • C23C16/463—Cooling of the substrate
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/44—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating
    • C23C16/50—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes characterised by the method of coating using electric discharges
    • C—CHEMISTRY; METALLURGY
    • C23—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; CHEMICAL SURFACE TREATMENT; DIFFUSION TREATMENT OF METALLIC MATERIAL; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL; INHIBITING CORROSION OF METALLIC MATERIAL OR INCRUSTATION IN GENERAL
    • C23C—COATING METALLIC MATERIAL; COATING MATERIAL WITH METALLIC MATERIAL; SURFACE TREATMENT OF METALLIC MATERIAL BY DIFFUSION INTO THE SURFACE, BY CHEMICAL CONVERSION OR SUBSTITUTION; COATING BY VACUUM EVAPORATION, BY SPUTTERING, BY ION IMPLANTATION OR BY CHEMICAL VAPOUR DEPOSITION, IN GENERAL
    • C23C16/00—Chemical coating by decomposition of gaseous compounds, without leaving reaction products of surface material in the coating, i.e. chemical vapour deposition [CVD] processes
    • C23C16/56—After-treatment
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/29—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials characterised by the substrates
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/20—Formation of materials, e.g. in the shape of layers or pillars of semiconductor materials
    • H10P14/34—Deposited materials, e.g. layers
    • H10P14/3402—Deposited materials, e.g. layers characterised by the chemical composition
    • H10P14/3404—Deposited materials, e.g. layers characterised by the chemical composition being Group IVA materials
    • H10P14/3411—Silicon, silicon germanium or germanium
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/63—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the formation processes
    • H10P14/6326—Deposition processes
    • H10P14/6328—Deposition from the gas or vapour phase
    • H10P14/6334—Deposition from the gas or vapour phase using decomposition or reaction of gaseous or vapour phase compounds, i.e. chemical vapour deposition
    • H10P14/6336—Deposition from the gas or vapour phase using decomposition or reaction of gaseous or vapour phase compounds, i.e. chemical vapour deposition in the presence of a plasma [PECVD]
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/66—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the type of materials
    • H10P14/668—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the type of materials the materials being characterised by the deposition precursor materials
    • H10P14/6681—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the type of materials the materials being characterised by the deposition precursor materials the precursor containing a compound comprising Si
    • H10P14/6682—Formation of materials, e.g. in the shape of layers or pillars of insulating materials characterised by the type of materials the materials being characterised by the deposition precursor materials the precursor containing a compound comprising Si the compound being a silane, e.g. disilane, methylsilane or chlorosilane
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P14/00—Formation of materials, e.g. in the shape of layers or pillars
    • H10P14/60—Formation of materials, e.g. in the shape of layers or pillars of insulating materials
    • H10P14/69—Inorganic materials
    • H10P14/692—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses
    • H10P14/6921—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses containing silicon
    • H10P14/69215—Inorganic materials composed of oxides, glassy oxides or oxide-based glasses containing silicon the material being a silicon oxide, e.g. SiO2
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P34/00—Irradiation with electromagnetic or particle radiation of wafers, substrates or parts of devices
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P34/00—Irradiation with electromagnetic or particle radiation of wafers, substrates or parts of devices
    • H10P34/40—Irradiation with electromagnetic or particle radiation of wafers, substrates or parts of devices with high-energy radiation
    • H10P34/42—Irradiation with electromagnetic or particle radiation of wafers, substrates or parts of devices with high-energy radiation with electromagnetic radiation, e.g. laser annealing
    • H10P34/422—Irradiation with electromagnetic or particle radiation of wafers, substrates or parts of devices with high-energy radiation with electromagnetic radiation, e.g. laser annealing using incoherent radiation
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P72/00—Handling or holding of wafers, substrates or devices during manufacture or treatment thereof
    • H10P72/04—Apparatus for manufacture or treatment
    • H10P72/0431—Apparatus for thermal treatment
    • H10P72/0436—Apparatus for thermal treatment mainly by radiation
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P72/00—Handling or holding of wafers, substrates or devices during manufacture or treatment thereof
    • H10P72/04—Apparatus for manufacture or treatment
    • H10P72/0451—Apparatus for manufacturing or treating in a plurality of work-stations
    • H10P72/0468—Apparatus for manufacturing or treating in a plurality of work-stations comprising a chamber adapted to a particular process
    • H—ELECTRICITY
    • H10—SEMICONDUCTOR DEVICES; ELECTRIC SOLID-STATE DEVICES NOT OTHERWISE PROVIDED FOR
    • H10P—GENERIC PROCESSES OR APPARATUS FOR THE MANUFACTURE OR TREATMENT OF DEVICES COVERED BY CLASS H10
    • H10P95/00—Generic processes or apparatus for manufacture or treatments not covered by the other groups of this subclass
    • H10P95/90—Thermal treatments, e.g. annealing or sintering

Definitions

  • This disclosure relates to a substrate processing method, a substrate processing apparatus, and a substrate processing system.
  • Patent Document 1 describes a technique for applying stress to a substrate by forming a dummy film having compressive stress, such as a SiO 2 film or a SiN film, on the rear surface of the substrate by ALD or CVD.
  • a dummy film having compressive stress such as a SiO 2 film or a SiN film
  • the present disclosure provides a technology that can generate large stress on a second surface of a substrate, opposite the first surface on which devices are formed.
  • the present disclosure provides a technology that can generate large stress on a second surface of a substrate, opposite the first surface on which devices are formed.
  • FIG. 3 is a flowchart showing a substrate processing method according to the first embodiment.
  • 3A to 3C are cross-sectional views illustrating process steps of a substrate processing method according to a first embodiment.
  • 3A to 3C are cross-sectional views illustrating process steps of a substrate processing method according to a first embodiment.
  • 4 is a cross-sectional view showing a base of a sample used in an experiment to confirm stress generated on a second surface of a substrate due to shrinkage of a silicon-containing film formed according to the first embodiment.
  • FIG. 4 is a cross-sectional view showing a sample used in an experiment to confirm stress generated on a second surface of a substrate, the sample being formed by depositing a silicon-containing film on the base of FIG. 3.
  • FIG. 5 is a diagram showing the relationship between the annealing temperature and the Raman shift when the sample of FIG. 4 is annealed.
  • FIG. 6 is a cross-sectional view showing a schematic stress state of the second surface of the substrate in an initial state (A in FIG. 5) before the silicon-containing film used to obtain the relationship in FIG. 5 is formed.
  • 5B and 5C are diagrams showing the stress on the second surface of the substrate when the annealing temperature is less than 100° C.
  • 5D is a diagram showing the stress on the second surface of the substrate when the annealing temperature is changed from 100° C. to 200° C. and the Raman shift changes to a positive value (FIG. 5D).
  • FIG. 5D is a diagram showing the relationship between the annealing temperature and the Raman shift when the sample of FIG. 4 is annealed.
  • FIG. 6 is a cross-sectional view showing a schematic stress state of the second surface of the substrate in an initial state (A in FIG. 5)
  • FIG. 1 is a cross-sectional view showing an example of a substrate processing apparatus used in carrying out a first embodiment.
  • 10 is a flowchart showing a substrate processing method according to a second embodiment.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a second embodiment of the present invention.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a second embodiment of the present invention.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a second embodiment of the present invention.
  • FIG. 11 is a plan view illustrating an example of a substrate processing system used in a second embodiment.
  • FIG. 13 is a cross-sectional view showing an example of an annealing apparatus used in the substrate processing system of FIG. 12.
  • 10 is a flowchart showing a substrate processing method according to a third embodiment.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a third embodiment.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a third embodiment.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a third embodiment.
  • 10A to 10C are cross-sectional views illustrating process steps of a substrate processing method according to a third embodiment.
  • FIG. 11 is a plan view illustrating an example of a substrate processing system used in a third embodiment.
  • 17 is a cross-sectional view showing a schematic diagram of a stress measuring device used in the substrate processing system of FIG. 16.
  • FIG. 1 is a flow chart showing a substrate processing method according to a first embodiment, and FIGS. 2A to 2B are cross-sectional views showing the steps.
  • a substrate 1 having a first surface 2 on which a device is to be formed is prepared (step ST1, FIG. 2A).
  • a high-order silane gas is supplied as a deposition gas to a second surface 3 opposite the first surface 2 of the substrate 1, and a silicon-containing film 4 is deposited at a temperature at which the high-order silane gas is liquefied (step ST2, FIG. 2B).
  • the substrate 1 is not particularly limited, but a typical example is a semiconductor substrate (wafer).
  • the first surface 2 of the substrate may or may not actually have a device formed thereon, and may be in the middle of forming a device.
  • step ST2 a high-order silane gas is used as the deposition gas, and a silicon-containing film 4 is deposited on the second surface 3 of the substrate 1 at a temperature at which the high-order silane gas liquefies.
  • the silicon-containing film 4 may be deposited on the entire surface of the second surface 3, or may be deposited on only a portion of the second surface 3.
  • Higher silane gas can be liquefied at a practical temperature of about -30°C.
  • a film is formed in which low molecular weight components remain in the film.
  • energy such as heat or light
  • a large amount of the components in the film vaporize, causing the film to aggregate and shrink significantly.
  • This shrinkage can generate large stress on the second surface 3 of the substrate 1.
  • the silicon-containing film 4 formed using higher silane gas at a temperature at which higher silane gas liquefies has a high stress generation ability for the substrate.
  • step ST2 can be performed, for example, by placing the substrate with its second side facing up on a mounting table in the chamber, holding the substrate on the mounting table at a temperature at which the high-order silane gas liquefies, and introducing the high-order silane gas into the chamber and supplying it to the second side of the substrate in a plasma-excited state.
  • the substrate can be held at a temperature at which the high-order silane gas liquefies, for example -30°C, by passing a coolant through the mounting table.
  • the pressure in the chamber at this time may be in the range of 10 Torr or less, for example 1 Torr.
  • the skeleton of the film is formed by gas phase polymerization even at low temperatures, and film formation can proceed. Furthermore, by using plasma, a film with high adhesion can be obtained.
  • plasma There are no particular limitations on the type of plasma, and various types such as capacitively coupled plasma, inductively coupled plasma, and microwave plasma can be used.
  • Higher silanes include disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), tetrasilane (Si 4 H 10 ), and the like, and are expressed by the general formula Si n H 2n+2 (n is a positive integer of 2 or more).
  • the boiling points of Si 2 H 6 , Si 3 H 8 , and Si 4 H 10 are ⁇ 14.5° C., 52.8° C., and 108.1° C., respectively, all of which are sufficiently higher than the boiling point of monosilane (SiH 4 ), which is ⁇ 112° C., and as described above, they can be stably liquefied at a realistic temperature of about ⁇ 30° C.
  • those with n of 4 or more can obtain a greater shrinking ability.
  • the gas used in the film formation may be H2 gas or a rare gas (e.g., Ar gas) as a plasma generating gas.
  • a rare gas e.g., Ar gas
  • the silicon-containing film is a Si-based film, and becomes a Si film after the vaporized components in the film are vaporized.
  • An oxygen-containing gas may be further added as the film formation gas to make the silicon-containing film a SiO2 - based film that finally becomes a SiO2 film. In this way, by changing the film quality of the silicon-containing film, the shrink characteristics change, and the ability to generate stress on the second surface of the substrate can be adjusted.
  • the silicon-containing film 4 has a large stress generating capability, so it can be thinner than films made by conventional CVD or ALD to generate the desired stress.
  • the thickness of the silicon-containing film 4 can be set appropriately according to the stress to be generated, and can be in the range of 1 to 10,000 nm.
  • tetrasilane was used as the high-order silane, which is the deposition gas, and the substrate was held on a stage in the chamber at -30°C, at which the high-order silane gas liquefies, and the high-order silane gas was excited by plasma and supplied to the substrate to deposit a silicon-containing film. The ability to generate stress on the second surface of the substrate was then investigated.
  • the substrate on which the silicon-containing film was formed on the stage was annealed at various temperatures, and the desorbed gas was analyzed by thermal desorption spectroscopy (TDS).
  • TDS thermal desorption spectroscopy
  • H 2 gas and silane-based gases such as SiH 4 , Si 2 H 6 , and Si 3 H 8 were desorbed.
  • the film structure change was confirmed by Fourier transform infrared spectroscopy (FT-IR). It was confirmed that the intensity of SiH x (SiH, SiH 2 , SiH 3 , (SiH 2 ) n , etc.) decreased as the annealing temperature increased. From these results, it was confirmed that the shrink of the silicon-containing film formed by this embodiment was caused by the desorption of H 2 gas and silane-based gas.
  • FIG. 3 a sample was created in which thermal oxide films 203, 204 were formed to a thickness of 100 nm on both the first surface 201 and the second surface 202 of a Si substrate 200, and as shown in FIG. 4, a silicon-containing film 205 was formed to a thickness of 50 nm on the thermal oxide film 204 on the second surface 202 side of the Si substrate 200.
  • the thermal oxide film was formed so that the silicon-containing film, which is a Si-based film, could be distinguished from the Si substrate.
  • the sample was annealed to grasp the stress generated on the second surface 202 of the substrate 200 due to shrinkage of the silicon-containing film 205.
  • the stress was measured by cross-sectional Raman measurement (Raman spectroscopy).
  • the stress generated on the substrate due to shrinkage of the silicon-containing film can be calculated based on the shift (Raman shift) from 520 (cm ⁇ 1 ), which is the peak of the Si crystal (crystal not subjected to stress) in the spectrum (Raman spectrum) of Raman scattered light.
  • FIG. 5 is a diagram showing the relationship between the annealing temperature and the Raman shift when the above sample was annealed.
  • the annealing time was about 1 hour at each temperature.
  • the Raman shift on the vertical axis is set to 0 at 520 (cm ⁇ 1 ), which is the silicon peak, with negative values indicating the tensile direction and positive values indicating the compressive direction. Note that the thermal oxide film relieves the substrate stress, but here the values are corrected to eliminate the influence of the thermal oxide film.
  • A is the value of the Raman shift in the initial state in which no silicon-containing film is formed for comparison, and the others are the values of the Raman shift in the state in which the silicon-containing film is formed and then annealed at a predetermined temperature.
  • the Raman shift of the substrate is ⁇ 0.4 cm ⁇ 1 . That is, in the initial state, as shown in FIG. 6, a tensile stress 210 of about 200 MPa is generated on the second surface 202 of the substrate 200. After the silicon-containing film 205 is formed, the Raman shift becomes slightly larger at ⁇ 0.5 cm ⁇ 1 , and the Raman shift remains negative when the annealing temperature is less than 100° C. (FIG. 5B, C). That is, as shown in FIG. 7, the tensile stress 210 remains generated on the second surface 202 of the substrate 200. However, the Raman shift changes significantly between the annealing temperature of 100° C.
  • the Raman shift becomes positive at 200° C. (FIG. 5D). That is, as shown in FIG. 8, the stress generated on the second surface 202 of the substrate 200 changes from the tensile stress 210 to the compressive stress 220. At annealing temperatures of 200° C. or higher, the Raman shift does not change significantly, but at 400° C., the Raman shift reaches a maximum value of +0.5 cm ⁇ 1 or more (FIG. 5E).
  • the Raman shift changes from about ⁇ 0.5 cm ⁇ 1 to +0.5 cm ⁇ 1 , and the amount of change is about 1.0 cm ⁇ 1 .
  • the stress is calculated from the amount of change in the Raman shift using formula (1), it becomes 500 MPa or more, and it was confirmed that an extremely large stress can be generated in a relatively thin film thickness of 50 nm.
  • the silicon-containing film formed on the substrate using a high-order silane gas as the deposition gas in this embodiment at a temperature at which the high-order silane liquefies is a film that can generate extremely large stress on the substrate.
  • the film formed on the second surface is deposited by typical CVD or ALD methods, which do not generate significant stress in the substrate, and the only solution is to increase the film thickness.
  • the compressive stress generated in the substrate can be somewhat increased by depositing the film at a high temperature, but the effect is limited, and deposition at high temperatures is generally restricted due to the impact on devices.
  • a high-order silane gas is used as the deposition gas, and a film is deposited on the second surface of the substrate at a temperature at which the high-order silane gas liquefies, thereby obtaining a silicon-containing film with high shrinkage capability.
  • This film can be significantly shrunk by annealing or the like, making it possible to impart large stress to the substrate.
  • the desired stress can be imparted to the substrate without thickening the film as occurs with films deposited by general CVD or ALD, and because the film is deposited at a low temperature, no inconveniences arise due to high-temperature deposition.
  • [Substrate Processing Apparatus] 9 is a cross-sectional view showing an example of a substrate processing apparatus used in carrying out the first embodiment.
  • the substrate processing apparatus 100 is configured as a film forming apparatus that forms a silicon-containing film at a low temperature on a second surface of a substrate W opposite to a first surface on which devices are formed, by capacitively coupled plasma.
  • the substrate processing apparatus 100 has a chamber 10 that is roughly cylindrical and defines a processing space 11.
  • the chamber 10 is made of metal, for example aluminum whose surface has been anodized, and is installed in a secure manner.
  • a cylindrical metal support table 14 is placed on the bottom of the chamber 10 via an insulating plate 12, and a mounting table 16 is provided on the support table 14 for mounting a substrate W made of a metal, such as aluminum.
  • the mounting table 16 constitutes a lower electrode.
  • the mounting table 16 has an electrostatic chuck 18 on its upper part.
  • the electrostatic chuck 18 has a structure in which an electrode 20 is provided inside an insulator, and by applying a DC voltage from an adsorption DC power supply 22 to the electrode 20, the substrate W is attracted and held by electrostatic forces such as Coulomb force.
  • the substrate W is placed on the mounting table 16 so that the second surface becomes the gas supply surface.
  • a refrigerant chamber 28 is provided inside the support table 14, and a low-temperature refrigerant is circulated and supplied to the refrigerant chamber 28 from an external chiller unit (not shown) via pipes 30a and 30b, so that the temperature of the substrate W on the mounting table 16 is controlled to a low temperature, for example -30°C, at which the high-order silane gas supplied as the film-forming gas liquefies.
  • a heat transfer gas for example He gas, is supplied between the upper surface of the electrostatic chuck 18 and the back surface of the substrate W via a gas supply line 32.
  • the upper electrode 34 is provided so as to face the mounting table 16.
  • the upper electrode 34 is supported on the upper part of the chamber 10 via an insulating shielding member 43.
  • the upper electrode 34 is composed of an electrode plate 36 that forms the surface facing the mounting table 16 and has a number of gas discharge holes 37, and an electrode support 38 with a water-cooled structure that supports the electrode plate 36 in a removable manner.
  • the electrode plate 36 is made of a conductor, for example, silicon.
  • a gas diffusion chamber 40 is provided inside the electrode support 38, and a number of gas flow holes 41 that communicate with the gas discharge holes 37 extend downward from the gas diffusion chamber 40.
  • a gas inlet 42 that introduces gas such as a film-forming gas to the gas diffusion chamber 40 is formed in the electrode support 38, and a gas pipe 51 extending from a gas supply unit 50 described later is connected to this gas inlet 42.
  • the upper electrode 34 is configured as a shower head that introduces gas such as a film-forming gas into the processing space 11.
  • a first high frequency power supply 88 for generating plasma is electrically connected to the upper electrode 34.
  • a matching box 87 is provided on a power supply line 89 that supplies power from the first high frequency power supply 88 to the upper electrode 34.
  • a second high frequency power supply 91 for applying a bias to attract ions to the substrate W is electrically connected to the lower electrode, the mounting table 16.
  • a matching box 90 is provided on a power supply line 92 that supplies power from the second high frequency power supply 91 to the lower electrode, the mounting table 16.
  • the matching boxes 87 and 90 are provided to match the load (plasma) impedance to the impedance on the first and second high frequency power supplies 88 and 91 sides, respectively.
  • the first high frequency power supply 88 for generating plasma has a higher frequency than the second high frequency power supply 91 for applying a bias.
  • the gas supply unit 50 supplies high-order silane gas, which is a film-forming gas for forming a silicon-containing film on the second surface of the substrate W.
  • the gas supply unit 50 also supplies a purge gas, a pressure-regulating gas, and a plasma generating gas consisting of a rare gas such as Ar gas.
  • H2 gas and an oxygen-containing gas may be supplied.
  • High-order silanes are represented by the general formula Si n H 2n +2 (n is a positive integer of 2 or more), such as Si 2 H 6 , Si 3 H 8 , and Si 4 H 10, and any of these can be used, but a film with a large shrink capacity can be obtained by using one in which n is 4 or more.
  • the gas supply unit 50 has gas supply sources corresponding to the multiple gases to be supplied, and individual pipes extending from each gas supply source are connected to a gas pipe 51. An opening/closing valve and a flow rate controller are interposed in each individual pipe.
  • An exhaust port 60 is provided at the bottom of the chamber 10, and an exhaust device 64 is connected to the exhaust port 60 via an exhaust pipe 62.
  • the exhaust device 64 includes an automatic pressure control valve and a vacuum pump, and evacuates the inside of the chamber 10 using the exhaust device 64 while controlling the vacuum level to the desired level.
  • a load/unload port 65 for loading/unloading the substrate W into/from the chamber 10 is provided on the side wall of the chamber 10, and the load/unload port 65 is opened and closed by a gate valve 66.
  • the substrate processing apparatus 100 has a control unit 70.
  • the control unit 70 is composed of a computer, and has a main control unit equipped with a CPU, an input device (keyboard, mouse, etc.), an output device (printer, etc.), a display device (display, etc.), and a storage device (storage medium).
  • the main control unit controls, for example, the high frequency power supplies 88, 91, the opening and closing valve of the gas supply unit 50, the flow rate controller, the automatic pressure control valve, the adsorption DC power supply 22, the chiller unit, the gate valve 66, etc.
  • These control operations by the main control unit are executed by a processing recipe, which is a control program stored in a storage medium (hard disk, optical disk, semiconductor memory, etc.) built into the storage device.
  • the substrate W is loaded into the chamber 10 and placed on the mounting table 16 with the second surface facing up. Then, an inert gas is supplied from the gas supply unit 50 into the chamber 10, and the pressure inside the chamber 10 is adjusted to a reduced pressure by the exhaust device 64.
  • a plasma generating gas for example Ar gas
  • Ar gas is supplied from the gas supply unit 50 into the chamber 10
  • a plasma generating high frequency power is applied from the first high frequency power source 88 to the upper electrode 34.
  • the plasma generating gas may be used as the inert gas for adjusting the pressure.
  • a bias applying high frequency power for attracting ions is applied to the mounting table 16 from the second high frequency power source 91.
  • high-order silane gas which is a film-forming gas
  • the gas supply unit 50 into the chamber 10, whereby the high-order silane gas is excited by plasma.
  • the excited high-order silane gas reaches the second surface of the substrate W, which is held at a temperature at which the high-order silane liquefies, for example, at -30°C, and film formation proceeds by gas-phase polymerization at this low temperature. This results in the formation of a silicon-containing film that has a high shrink capacity as described above and can generate large stress on the second surface of the substrate W.
  • FIG. 10 is a flow chart showing a substrate processing method according to the second embodiment, and FIGS. 11A to 11C are cross-sectional views showing the steps.
  • a substrate 1 having a first surface 2 on which a device is to be formed is prepared (step ST11, FIG. 11A).
  • a high-order silane gas is supplied as a deposition gas to a second surface 3 opposite the first surface 2 of the substrate 1, and a silicon-containing film 4 is deposited at a temperature at which the high-order silane gas is liquefied (step ST12, FIG. 11B).
  • energy 5 is applied to the silicon-containing film 4, generating stress 6 on the second surface 3 of the substrate 1 (step ST13, FIG. 11C).
  • steps ST11 and ST12 are performed in the same manner as steps ST1 and ST2 in the first embodiment.
  • step ST13 energy 5 is applied to the silicon-containing film 4 to generate stress 6 on the second surface 3 of the substrate 1. That is, by applying energy to the silicon-containing film 4, the silicon-containing film 4 shrinks, and the force generated by this shrinkage generates stress 6 on the second surface 3 of the substrate 1.
  • the silicon-containing film 4 has a high shrinking ability and can generate a large stress.
  • the method of applying energy to the silicon-containing film 4 is not particularly limited, and thermal energy, light energy, etc. can be used.
  • step ST13 by adjusting the amount of energy applied to the silicon-containing film 4, the amount of shrinkage of the silicon-containing film 4 can be adjusted, and the stress generated on the second surface 3 of the substrate 1 can be adjusted.
  • Annealing can be used as a method of providing energy to the silicon-containing film. During annealing, for example, the amount of energy can be adjusted by adjusting the annealing temperature and/or annealing time, thereby adjusting the stress.
  • the annealing can be thermal annealing or light annealing. Annealing can be performed using various devices such as a resistive heating element, a heat lamp, an LED, or a UV light source.
  • the annealing temperature can be 100 to 400°C, and is particularly effective at 100 to 200°C.
  • the annealing time can be 10 seconds to 12 hours, for example, about 1 hour.
  • step ST13 energy may be applied to the entire silicon-containing film 4, or may be applied locally to the silicon-containing film 4. Applying energy to the entire film causes the silicon-containing film 4 to shrink overall, generating stress over the entire surface of the second surface 3 of the substrate 1. Applying energy locally causes only the portion of the silicon-containing film 4 to which energy has been applied to shrink, generating stress locally only in the portion of the second surface 3 of the substrate 1 that corresponds to that portion. Generating stress locally in this manner can alleviate local stress present on the first surface 2 of the substrate 1, for example.
  • the silicon-containing film 4 may be left or removed after generating stress on the second surface 3 of the substrate 1. That is, the silicon-containing film 4 may become unnecessary after generating stress on the substrate 1 and forming a device on the first surface 2, but leaving it will not adversely affect the device, and leaving it will save the trouble of removing it.
  • the silicon-containing film 4 can be easily removed when it is removed, and has the advantage that the entire film can be made thinner and flatness can be improved by removing it. Therefore, it is sufficient to decide whether to leave the silicon-containing film 4 or to remove it according to the requirements at the time of device formation.
  • a step of removing the silicon-containing film 4 is performed after a step of applying energy 5 to the silicon-containing film 4 to generate stress 6 on the second surface 3 of the substrate 1 (step ST13).
  • FIG. 12 is a plan view showing an example of a substrate processing system used in carrying out the second embodiment.
  • the substrate processing system 300 shown in Fig. 12 is a cluster structure (multi-chamber type) system, and includes a substrate processing apparatus 310, an annealing apparatus 320, a transfer chamber 330, a transfer apparatus 340, a load lock chamber 350, a loader module 360, and an overall control unit 370.
  • the substrate processing apparatus 310 supplies a high-order silane gas as a film-forming gas to the second surface of the substrate W at a temperature at which the high-order silane gas is liquefied, and forms a silicon-containing film on the second surface, and may be configured in the same manner as the substrate processing apparatus 100 of the first embodiment.
  • the annealing device 320 anneals the silicon-containing film formed on the second surface of the substrate to impart energy to the silicon-containing film and generate stress on the second surface of the substrate W.
  • An example of the annealing device 320 will be described later.
  • the transfer chamber 330 is maintained at a predetermined vacuum atmosphere, and is provided with a transfer device 340 that transfers the substrate W inside.
  • the transfer chamber 330 is connected to the above-mentioned substrate processing device 310 and annealing device 320, as well as the load lock chamber 350, via a gate valve (not shown).
  • the transfer device 340 transfers the substrate W between the substrate processing device 310, the annealing device 320, and the load lock chamber 350.
  • the load lock chamber 350 is provided between the loader module 360 and the transfer chamber 330, and is capable of switching between an atmospheric atmosphere and a vacuum atmosphere.
  • the loader module 360 is connected to the load lock chamber 350 via a gate valve (not shown) and is arranged adjacent to it, has an atmospheric atmosphere, and is provided with a transfer device (not shown).
  • a load port is provided on the wall of the loader module 360 opposite the load lock chamber 350, and a carrier (e.g., a FOUP (Front Opening Unified Pod)) containing or empty a substrate W is attached to the load port.
  • the transfer device of the loader module 360 transfers the substrate W between the load lock chamber 350 and the carrier attached to the load port.
  • the flow path forming member 130 is formed in a disk shape with approximately the same diameter as the top plate 120, and is made of a material transparent to the wavelength of light from the LED described below.
  • a groove for flowing the temperature control medium is formed in the upper part of the flow path forming member 130, and the groove is covered by the top plate 120 to become the temperature control medium flow path R.
  • a supply port 132 for supplying the temperature control medium to the temperature control medium flow path R and a discharge port 133 for discharging the temperature control medium are formed in the side of the flow path forming member 130, and a temperature control medium supply pipe 150 and a temperature control medium discharge pipe 151 are connected to these, respectively, and the temperature control medium is circulated and supplied to the temperature control medium flow path R.
  • a valve 152 is provided on the temperature control medium supply pipe 150.
  • the heating mechanism 140 is configured as a light irradiation mechanism, and is disposed so as to face the surface of the mounting table 110 opposite the substrate mounting surface, i.e., the underside of the flow path forming member 130, and correspond to the substrate W mounted on the top plate 120.
  • the heating mechanism 140 has a plurality of LEDs 141 as a heat source, and irradiates the top plate 120 of the mounting table 110 with light from the LEDs, thereby heating the silicon-containing film of the substrate W mounted thereon via the top plate 120.
  • Each LED 141 emits, for example, near-infrared light.
  • the light emitted from the LED 141 passes through the flow path forming member 130 of the mounting table 110, which is made of a light-transmitting material.
  • the temperature control medium flowing through the temperature control medium flow path R is made of a material that transmits the light from the LED 141, and the light that passes through the flow path forming member 130 and the temperature control medium is incident on the top plate 120.
  • polycarbonate, quartz, polyvinyl chloride, acrylic resin, or glass can be used as the light-transmitting material that constitutes the flow path forming member 130.
  • the heating mechanism 140 is configured by arranging multiple LED units 143, each of which is a unit made up of multiple LEDs 141 arranged as heat sources, with almost no gaps between them on the base portion 142.
  • Each LED unit 143 can be independently controlled for on/off and light intensity, making it possible to heat the substrate W uniformly or locally.
  • the annealing temperature of the substrate W can be controlled.
  • a refrigerant flow path may be provided in the base portion 142 so that the substrate can be cooled by a refrigerant.
  • the control unit 160 is composed of a computer, and has a main control unit with a CPU, an input device (keyboard, mouse, etc.), an output device (printer, etc.), a display device (display, etc.), and a storage device (storage medium).
  • the main control unit controls the on/off and light intensity of the LEDs 141 for each LED unit 143, and controls the flow rate of the temperature adjustment medium.
  • These control operations by the main control unit are executed by a processing recipe, which is a control program stored in a storage medium (hard disk, optical disk, semiconductor memory, etc.) built into the storage device.
  • the annealing device 320 configured in this manner can perform an annealing process on the entirety or locally on the silicon-containing film formed on the second surface of the substrate W, shrinking the silicon-containing film and generating stress on the entirety or locally on the second surface of the substrate W.
  • the above-mentioned substrate processing system 300 is an example in which a device for depositing a silicon-containing film and a device for annealing to generate stress are connected to a transfer chamber in a cluster structure, and the processing is performed in situ using these devices, but the present invention is not limited to this, and the substrate processing system may be configured by providing these devices separately.
  • the annealing device is not limited to one that uses an LED, and a resistive heating element, a heat lamp, or a UV light source may also be used.
  • the annealing device is not limited to one that uses an LED, and any device that can impart energy to the silicon-containing film may be used.
  • FIG. 14 is a flowchart showing a substrate processing method according to the third embodiment, and FIGS. 15A to 15D are cross-sectional views showing the processes.
  • a substrate 1 having a first surface 2 on which a device is formed is prepared (step ST21, FIG. 15A).
  • the stress distribution on the second surface 3 opposite to the first surface 2 of the substrate 1 is measured (step ST22).
  • This stress distribution measurement may be performed on the entire surface of the second surface 3 of the substrate 1, or may be performed on a part of the surface.
  • the stress distribution measurement may be performed, for example, by scanning the stress measurement unit 7 on the second surface 3 of the substrate 1, as shown in FIG. 15B.
  • a high-order silane gas is supplied as a film-forming gas to the second surface 3 of the substrate 1, and a silicon-containing film 4 is formed at a temperature at which the high-order silane gas is liquefied (step ST23, FIG.
  • step ST24 energy 5 is locally applied to the silicon-containing film 4 according to the stress distribution measured in step ST22, and a local stress 6 is generated on the second surface 3 of the substrate 1 so that the measured stress distribution is alleviated (step ST24, FIG. 15D).
  • steps ST21 and ST23 are performed in the same manner as steps ST1 and ST2 in the first embodiment.
  • the method of measuring the stress distribution on the second surface 3 of the substrate 1 is not particularly limited, but a measurement by Raman spectroscopy can be used.
  • the stress of the substrate 1 can be calculated by the above formula (1) from the shift amount (Raman shift) from 520 (cm ⁇ 1 ), which is the peak of a Si crystal (crystal not subjected to stress), by irradiating the substrate 1 with laser light to obtain the spectrum (Raman spectrum).
  • the stress distribution on the second surface 3 of the substrate 1 can be measured by scanning the second surface 3 with laser light using a stress measuring unit having a laser light source, an objective lens, a spectrometer, a detector, etc.
  • the stress distribution can be obtained by scanning the second surface 3 of the substrate 1 with laser light, measuring the Raman spectrum from the Raman scattered light, obtaining the Raman shift of the silicon peak at each position on the second surface 3 of the substrate 1, and calculating the stress at each position.
  • step ST24 based on the stress distribution on the second surface 3 of the substrate 1 measured in step ST22, energy is locally applied to the silicon-containing film 4 to shrink it, and stress is generated on the second surface 3 of the substrate 1 so as to alleviate the measured stress distribution. That is, in step ST24, energy is locally applied to the silicon-containing film 4 at the location on the second surface 3 of the substrate 1 where the stress was measured, so that stress is generated to alleviate the stress distribution.
  • a method for locally applying energy in this way for example, local annealing using an LED as described above can be used. Alternatively, local annealing may be performed by scanning a UV light source or a heat lamp.
  • the stress distribution on the second surface 3 of the substrate 1 is measured, and then the silicon-containing film 4 with a large shrink capacity as described above is formed, and annealing or the like is performed locally on the silicon-containing film 4 according to the stress distribution.
  • This local annealing or the like causes the annealed portion of the silicon-containing film 4 to shrink, which generates local stress on the second surface 3 of the substrate 1 so as to alleviate the measured stress distribution of the substrate.
  • non-uniformly distributed stress can be relieved by a simple method of simply performing annealing or the like according to the measured stress distribution.
  • large stress can be generated by shrinking the silicon-containing film, and the magnitude of the generated stress can be adjusted, so the stress relaxation effect in response to non-uniform stress distribution is large.
  • FIG. 16 is a plan view showing an example of a substrate processing system used in the implementation of the third embodiment.
  • the substrate processing system 400 shown in Fig. 16 is a cluster structure (multi-chamber type) system, and includes a substrate processing apparatus 410, an annealing apparatus 420, a stress measuring apparatus 480, a transfer chamber 430, a transfer apparatus 440, a load lock chamber 450, a loader module 460, and an overall control unit 470.
  • the substrate processing apparatus 410 supplies a high-order silane gas as a film-forming gas to the second surface of the substrate W at a temperature at which the high-order silane gas is liquefied, and forms a silicon-containing film on the second surface of the substrate W, and may be configured similarly to the substrate processing apparatus 100 of the first embodiment.
  • the annealing device 420 locally anneals the silicon-containing film formed on the second surface of the substrate W in accordance with the stress distribution measured by the stress measuring device 480 described below, thereby generating local stress on the second surface of the substrate W so as to relieve the measured stress.
  • the annealing device 420 may be configured similarly to the annealing device 320 of the second embodiment, which is capable of local annealing.
  • the stress measuring device 480 has, as shown in FIG. 17, a stage 501 on which the substrate W is placed, a laser light source 502, an objective lens 503, a spectrometer 504, a multichannel detector 505 for measuring the spectrum, and a control unit 506.
  • the substrate W is placed on the stage 501 with the second surface facing up.
  • the stage 501 is freely movable within a plane, and the laser light can be scanned on the second surface of the substrate W.
  • the laser light may be scanned by moving the optical system.
  • the laser light from the laser light source 502 is irradiated onto the second surface of the substrate W via the objective lens 503.
  • the Raman scattered light generated from the second surface of the substrate W is collected by the objective lens 503 and guided to the spectrometer 504, and the Raman spectrum is measured by the multichannel detector 505.
  • the control unit 506 controls each component of the stress measuring device 480 and functions as a calculation unit, and the control unit 506 determines the Raman shift of the silicon peak from the Raman spectrum to calculate the stress.
  • the transfer chamber 430 is maintained at a predetermined vacuum atmosphere, and is provided with a transfer device 440 that transfers the substrate W inside.
  • the transfer chamber 430 is connected to the above-mentioned substrate processing apparatus 410, annealing apparatus 420, stress measuring apparatus 480, and load lock chamber 450 via a gate valve (not shown).
  • the transfer device 440 transfers the substrate W between the substrate processing apparatus 410, annealing apparatus 420, stress measuring apparatus 480, and load lock chamber 450.
  • the load lock chamber 450 and the loader module 460 are configured similarly to the load lock chamber 350 and the loader module 360 of the substrate processing system 300 of the second embodiment.
  • the loader module 460 is provided with a transport device, which transports the substrate W between the load lock chamber 450 and a carrier attached to the load port.
  • the overall control unit 470 is configured as a computer, and is configured similarly to the overall control unit 370 in the substrate processing system 300 of the second embodiment, and controls the processing of the substrate processing apparatus 410, the annealing apparatus 420, and the stress measuring apparatus 480, the transport apparatus 440 and the transport apparatus of the loader module 460, and the opening and closing of the gate valve.
  • the overall control unit 470 also stores the stress distribution measured by the stress measuring apparatus 480, and accordingly issues a command to the annealing apparatus 420 regarding the portion to be annealed.
  • the overall control unit 470 may be configured as a higher-level control unit of the control units of the substrate processing apparatus 410, the annealing apparatus 420, and the stress measuring apparatus 480.
  • a substrate W is removed from a carrier connected to a load port by a transport device (not shown) in the loader module 460, and is transported into the load lock chamber 450 in an atmospheric environment.
  • the substrate W may have a device formed on its first surface, or may have a pattern formed in the middle of device formation.
  • the load lock chamber 450 is set to a vacuum atmosphere, and the substrate W in the load lock chamber 450 is transported by the transport device 440 to the stress measuring device 480 with the second surface facing up.
  • the stress measuring device 480 measures the stress distribution over the entire or part of the second surface of the substrate W.
  • the measurement result of the stress distribution is stored in the overall control unit 470.
  • the substrate W whose stress distribution has been measured is then transported by the transport device 440 from the stress measuring device 480 and transported to the substrate processing device 410.
  • a high-order silane gas as a film-forming gas is supplied to the second surface of the substrate W at a temperature at which the high-order silane gas is liquefied, and a silicon-containing film is formed on the second surface.
  • the substrate W on which the silicon-containing film has been formed is then transported by the transport device 440 from the substrate processing device 410 and transported to the annealing device 420.
  • the annealing device 420 local annealing is performed on the silicon-containing film 4 according to the stress distribution measurement result of the stress measuring device 480 stored in the overall control unit 470.
  • This local annealing causes the annealed portion of the silicon-containing film to shrink, generating local stress on the second surface of the substrate W so as to alleviate the stress distribution of the substrate W measured by the stress measuring device 480.
  • the annealed substrate W is then removed by the transport device 440 and transported to the load lock chamber 450.
  • the above-mentioned processing is carried out simultaneously in parallel for multiple substrates W, completing the processing of multiple substrates W in the carrier.
  • the above-mentioned substrate processing system 400 is an example in which a device for depositing a silicon-containing film, a device for annealing to generate stress, and a stress measurement device are connected to a transfer chamber in a cluster structure, and the processing is performed in situ using these devices, but the present invention is not limited to this, and the substrate processing system may be configured by providing these devices separately.
  • the annealing device is not limited to one that uses an LED, and any device that can perform localized heating may be used, such as a UV light source or a heat lamp.
  • the device is not limited to an annealing device, and any device that can provide energy to the silicon-containing film may be used.
  • a Si film and a SiO 2 film are exemplified as the silicon-containing film formed on the second surface of the substrate, but the present invention is not limited to these and may be other Si-containing films such as a SiN film.
  • the substrate processing apparatus for forming a silicon-containing film is exemplified as an apparatus in which the substrate is cooled by a mounting table and processed using capacitively coupled plasma, but the present invention is not limited to this.
  • the substrate cooling method is not limited to a method of cooling by a mounting table, as long as the film can be formed at a temperature at which the high-order silane gas liquefies.
  • the plasma is not limited to capacitively coupled plasma, and may be inductively coupled plasma, microwave plasma, or remote plasma.
  • the film may be formed using a method that does not use plasma, as long as the film can be formed at a temperature at which the high-order silane gas liquefies.
  • the annealing device and stress measuring device are merely examples, and their configurations are not limited as long as they can achieve the intended purpose.

Landscapes

  • Chemical & Material Sciences (AREA)
  • Engineering & Computer Science (AREA)
  • Mechanical Engineering (AREA)
  • Chemical Kinetics & Catalysis (AREA)
  • General Chemical & Material Sciences (AREA)
  • Materials Engineering (AREA)
  • Metallurgy (AREA)
  • Organic Chemistry (AREA)
  • Inorganic Chemistry (AREA)
  • Physics & Mathematics (AREA)
  • Plasma & Fusion (AREA)
  • Chemical Vapour Deposition (AREA)
  • Formation Of Insulating Films (AREA)
PCT/JP2024/042503 2023-12-14 2024-12-02 基板処理方法、基板処理装置、および基板処理システム Pending WO2025126879A1 (ja)

Priority Applications (1)

Application Number Priority Date Filing Date Title
KR1020267021301A KR20260121466A (ko) 2023-12-14 2024-12-02 기판 처리 방법, 기판 처리 장치, 및 기판 처리 시스템

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
JP2023210808A JP2025095041A (ja) 2023-12-14 2023-12-14 基板処理方法、基板処理装置、および基板処理システム
JP2023-210808 2023-12-14

Publications (1)

Publication Number Publication Date
WO2025126879A1 true WO2025126879A1 (ja) 2025-06-19

Family

ID=96057120

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/JP2024/042503 Pending WO2025126879A1 (ja) 2023-12-14 2024-12-02 基板処理方法、基板処理装置、および基板処理システム

Country Status (3)

Country Link
JP (1) JP2025095041A (enExample)
KR (1) KR20260121466A (enExample)
WO (1) WO2025126879A1 (enExample)

Families Citing this family (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP7924541B1 (ja) 2025-07-29 2026-09-25 ATI Japan 株式会社 酸化シリコン膜をもつ基板の製造方法

Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63207121A (ja) * 1987-02-23 1988-08-26 Nikon Corp 光cvdによる薄膜の製造方法及びそれに使用される装置
JP2004318165A (ja) * 1996-05-15 2004-11-11 Seiko Epson Corp 薄膜デバイスの製造方法、薄膜トランジスタの形成方法、及び電子機器の製造方法
JP2016021503A (ja) * 2014-07-15 2016-02-04 独立行政法人国立高等専門学校機構 ゲルマニウム層付き基板の製造方法及びゲルマニウム層付き基板
JP2016510507A (ja) * 2013-01-25 2016-04-07 アプライド マテリアルズ インコーポレイテッドApplied Materials,Incorporated 低収縮性誘電膜
JP2016086152A (ja) * 2014-03-27 2016-05-19 Sppテクノロジーズ株式会社 シリコン酸化膜及びその製造方法、並びにシリコン酸化膜の製造装置

Family Cites Families (1)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP2020150133A (ja) 2019-03-13 2020-09-17 東京エレクトロン株式会社 基板処理方法及び基板処理装置

Patent Citations (5)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPS63207121A (ja) * 1987-02-23 1988-08-26 Nikon Corp 光cvdによる薄膜の製造方法及びそれに使用される装置
JP2004318165A (ja) * 1996-05-15 2004-11-11 Seiko Epson Corp 薄膜デバイスの製造方法、薄膜トランジスタの形成方法、及び電子機器の製造方法
JP2016510507A (ja) * 2013-01-25 2016-04-07 アプライド マテリアルズ インコーポレイテッドApplied Materials,Incorporated 低収縮性誘電膜
JP2016086152A (ja) * 2014-03-27 2016-05-19 Sppテクノロジーズ株式会社 シリコン酸化膜及びその製造方法、並びにシリコン酸化膜の製造装置
JP2016021503A (ja) * 2014-07-15 2016-02-04 独立行政法人国立高等専門学校機構 ゲルマニウム層付き基板の製造方法及びゲルマニウム層付き基板

Also Published As

Publication number Publication date
KR20260121466A (ko) 2026-08-11
JP2025095041A (ja) 2025-06-26

Similar Documents

Publication Publication Date Title
KR102920126B1 (ko) 국부적인 응력 변조를 위한 uv 경화
US20210010160A1 (en) Method and apparatus for precleaning a substrate surface prior to epitaxial growth
KR102436174B1 (ko) 피처리체를 처리하는 방법
US12131913B2 (en) Methods, systems, and apparatus for processing substrates using one or more amorphous carbon hardmask layers
KR102464720B1 (ko) 비대칭 웨이퍼 보우 보상
JP2020002452A (ja) 選択的に膜を形成する方法およびシステム
TWI913723B (zh) 用於形成過渡金屬材料的群集處理系統
US12604687B2 (en) Large-area/wafer-scale CMOS-compatible 2D-material intercalation doping tools, processes, and methods, including intercalation doping of synthesized and patterned graphene
US20090104541A1 (en) Plasma surface treatment to prevent pattern collapse in immersion lithography
US7700376B2 (en) Edge temperature compensation in thermal processing particularly useful for SOI wafers
TW200847269A (en) Substrate processing apparatus
JP2025095041A (ja) 基板処理方法、基板処理装置、および基板処理システム
US20070105373A1 (en) Method of direct deposition of polycrystalline silicon
JP4545955B2 (ja) 半導体製造装置及び半導体装置の製造方法
KR20250069618A (ko) 반도체 기판을 위한 후면 층
US9721766B2 (en) Method for processing target object
CN116804270A (zh) 二氧化硅薄膜的低温沉积方法及器件制备方法
US12334317B2 (en) Remote plasma ultraviolet enhanced deposition
KR20150097431A (ko) 근적외선을 이용한 그래핀의 제조 방법 및 이를 위한 장치
KR102970792B1 (ko) 수소 함량이 감소된 규소 함유 층들 및 이들을 제조하는 프로세스들
WO2026155797A1 (en) Spatial varying laser technique for wafer shape and overlay correction
KR20240107965A (ko) 기판처리장치 및 기판처리방법
JP2003218046A (ja) 発熱体cvd装置及びこれを用いた発熱体cvd方法
WO2010070981A1 (ja) 半導体製造方法と装置
JP2603909C (enExample)

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 24903537

Country of ref document: EP

Kind code of ref document: A1

ENP Entry into the national phase

Ref document number: 1020267021301

Country of ref document: KR

Free format text: ST27 STATUS EVENT CODE: A-0-1-A10-A15-NAP-PA0105 (AS PROVIDED BY THE NATIONAL OFFICE)

WWE Wipo information: entry into national phase

Ref document number: 1020267021301

Country of ref document: KR

NENP Non-entry into the national phase

Ref country code: DE

WWP Wipo information: published in national office

Ref document number: 1020267021301

Country of ref document: KR